Maggie Moo's Blue-Green glaze #5
This glaze recipe is adapted from a combination of a Mastering Cone 6 Glazes base glaze and Maggie Schlebecker's blue-green glaze recipe. It is cone 6 oxidation.You can adjust the percentage of copper, tin, and zinc to produce a range of color from a pale mint to a deep sea green. Varying the amount of tin and zinc will affect the opacity of the glaze and make it milkier the more you add. Overdoing it on the copper could cause leaching, so going over 5% is probably not a good idea, but otherwise this base is extremely stable and food safe.
Custer Spar 20.0 (kaliveldspaat)
Ferro Frit 3134 20.0
Wollastonite 10.0
EPK 21.0 (kaoline)
Talc 11.5
Silica 17.5 (kwarts SiO2)
------------
Total 100.0
Add
Tin Oxide 3.96
Zinc Oxide 2.45
Copper Carb 3.21 (or Black Copper Oxide 2.14)