Hour hold at 1650 F,
Recipe Name: C HARRIS TEMMOKU
Cone:  6     Color:  TEMMOKU
Firing:  Oxidation     Surface:  Glossy
Amount     Ingredient
18.6          Nepheline Syenite
8.5          Gerstley Borate--1999
9.3          Dolomite
9.3          Talc
18.6          Ball Clay Number 1
28.2          Silica
7.5          Bone Ash
100 Total
               Additives
11          Iron Oxide--Red
Unity          Oxide
.104           Na2O
.032           K2O
.359           MgO
.505           CaO
1.000          Total
.323           Al2O3
.094           B2O3
.005           Fe2O3
2.907           SiO2
.008           TiO2
.067           P2O5
9          Ratio
61            Exp
Comments:  
-----------------------------------
Calculations by GlazeMaster™
www.masteringglazes.com
------------------------------------
Tags:
Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase
Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com
Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.
Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.
The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.
Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .
If you are up to creating videos of your work or techniques you might want to invest in a flip video camera
Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00
And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62
ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.
If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014
    © 2025               Created by Andrea Wolf.             
    Powered by
    