Hour hold at 1650 F,

 

Recipe Name:  C HARRIS TEMMOKU

Cone:  6     Color:  TEMMOKU
Firing:  Oxidation     Surface:  Glossy

Amount     Ingredient
18.6          Nepheline Syenite
8.5          Gerstley Borate--1999
9.3          Dolomite
9.3          Talc
18.6          Ball Clay Number 1
28.2          Silica
7.5          Bone Ash

100         Total

               Additives
11          Iron Oxide--Red

Unity          Oxide
.104           Na2O
.032           K2O
.359           MgO
.505           CaO
1.000          Total

.323           Al2O3
.094           B2O3
.005           Fe2O3

2.907           SiO2
.008           TiO2
.067           P2O5

9          Ratio
61            Exp

Comments: 
-----------------------------------
Calculations by GlazeMaster™
www.masteringglazes.com
------------------------------------

Views: 2961

Replies to This Discussion

Your test looks very good. I've fired it on my pots on 3 or 4 occasions and it has alway come out looking great. I sprayed jens juicy fruit around the perimeter of a couple of plates and it seemed to make the c harris in the middle lose some of the red's intensity (more brown in it), but it may have been a fluke of firing as well. I'm down firing manually. How do you feel about your test? This is a gorgeous glaze in my opinion.
George I have been looking for this glaze for a long time. Do you know any glazes that either layer with this glaze good or other glazes that look good with it?
George I wonder if I add some other oxides I can get a semi matt black out of this glaze?
You could add 2% cobalt ox and 4% manganese dioxide for black. Make a test batch of that. Then use it to run a Fast-five glaze test with alumina hydrate or calcined alumina to find the amount that gets you a level of mattness you're looking for. With just the colorants, I would expect it to stay glossy. I doubt that you would have to use more than 10% alumina to start losing some of the gloss.
Take a look at my photos and let me know if you like any of the combinations there. I think I have photos of everything I've done with C. Harris so far, but I should have new tests out next week.
For the record, my recipe is slightly different, though the differences do not appear to make much difference. This is the recipe I used on all the pieces in my photos.
Recipe Name: C Harris Temoku

Cone: 6 Color: red brown black
Firing: Oxidation Surface: Glossy

Amount Ingredient
27.8 Silica
18.6 Kaolin--EPK
18.6 Nepheline Syenite
9.2 Gerstley Borate--1999
9.2 Dolomite
9.2 Talc
7.4 Bone Ash

100 Total

Additives
11.1 Iron Oxide--Red

Unity Oxide
.104 Na2O
.03 K2O
.356 MgO
.509 CaO
1.000 Total

.355 Al2O3
.102 B2O3
.004 Fe2O3

2.729 SiO2
.002 TiO2
.067 P2O5

7.7 Ratio
6.1 Exp

Comments: Posted on Clayart 1999 by C Harris as a temoku suitable for electric firing. I have a favorite ^6 glaze (C.Harris Tenmoku from the archives) that is it's very best when slow cooled and held at around 1850 for an hour or more.  Pete Pinnell wrote about some tomato red glazes that also profit from slow cool and long holds.
-----------------------------------
Calculations by GlazeMaster™
www.masteringglazes.com
------------------------------------

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service