does anyone have any idea what this beautiful glaze is? I love how it interacts with the clay body.


Views: 2924

▶ Reply to This

Replies to This Discussion

Sometimes white clay can flash orange in a wood firing.

that makes sense. thanks.

Thank you!

It looks like a typical copper, high barium carbonate matt.

June

A high sodium glaze will flash orange like this (the soda in the glaze interacting with the iron in the clay body) even in oxidation.  Pinnell's weathered bronze green does this but it is not similar enough in other aspects.  There are a couple of glazes close to this in color in the "Glaze Recipe Sharing" document in the FB group "Ceramic Recipes".  Perhaps if you took one of those recipes and replaced the feldspar with Neph Sye...

 

 This is

^6 Oxidation Chun Green (I would add 5-10% Tin or Zircopax to get the opaque look).  .

  • F-4 Feldspar 38

  • Whiting 14

  • Zinc Oxide 12

  • Ball Clay 6

  • Flint 30

  • 100

  •  

  • Celadon: copper Carbonate 1-2%

Donna Kat---saw in your post about a FB group named Ceramic Recipes???  how would One join this group?

Replacing the potspar with Neph sy will affect the firing range, because the Neph Sy has a stronger melt. It's balance of alumina and silica is different than a potspar and may affect the outcome in other ways as well.

Ian Currie has a barium looking glaze for cone 6 that looks a lot like the glaze in question and that may be worth a test. His glaze looks like a typical Barium matt, copper blue, but without barium. I have that glaze and recipe posted on my web site in one of the cone 6 test tile pages.http://www.shambhalapottery.com

Just hit technical links on the home page, and from there select the glaze pages.

June

Here's the late Ian Currie's recipe for a cone 6 matt glaze which mimics a traditional, copper blue barium matt usually seen at cone 10. With the colorant additions as shown, it will give a much deeper brighter blue. But if you try a variation and only add 1% copper carb, you might just get a color similar to this. On my web page, in the cone 10 glaze tests section, you can see a Carlton Ball barium copper matt which looks exactly like this glaze. It only has 1% copper, no iron, no cobalt. It's a Neph Sy, barium, copper, kaolin, silica recipe which I have listed on that page.

#7329 Brilliant Blue

 8.9 Soda Ash

8.0 Ferro Frit 3134

37.5 Nepheline Syenite

 2.4 Lithium Carbonate

17.7 Strontium carbonate

20.8 EPK

 4.7 Flint

A: add 3% Copper Carbonate  0.2% Cobalt Carbonate (this will be a deeper, richer color; but trying just 1% copper and eliminating the cobalt , you could probably get this.

Since a picture is worth a thousand words, that 2nd tile from the left is the Carlton Ball cone 10 Barium, copper matt that I have on my web site. The tile to the right of it is also a copper, barium, matt - a Vivika Heino recipe.

Sorry, missed this post.  On FB just do a search for Ceramic Recipes and it should come up.  I can give a link but I am not sure it will work. http://www.facebook.com/?ref=logo#!/groups/disisdkat/?bookmark_t=group - then just request to join.  It is an open group but you still have to make the request for some reason

It is really nice to see you posting again June.  Wonderful tiles as always. 

 

May I add this comment to the Ceramic Recipes Group?  It is the type of information the page needs.

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service