There are a number of glaze tests on my web site in the Potters Corner if anyone is interested.  Many tiles are layered glazes some of which are commerical glazes I have tested plus many others.  Pictures are included.

 

Make sure you scroll down past advertizements at top of page.

Views: 4237

▶ Reply to This

Replies to This Discussion

Hello Randy, I was looking at the replies and I notice the Randy Red glaze.  What is RIO and is there an alternative for it since I don't have any of it???

RIO is red iron oxide- gotta have it for this glaze.

Thanks a ton, Red Iron Oxide I have.  Can you send me the recipe again, I was just jumping from forum to forums and I'm not sure how to get back to where the recipe was..  Thanks

Randy's Red
Flint-30%
EPK-5%
G200-20%
Talc-15%
Gertsley borate-30%
RIO-15%

Should I come over and mix it for you, too?    Just kidding, really, I couldn't help myself :)

When I fire this glaze, on the cool down I hold it for 1 hour at 1650 degrees F after slow cooling from 1900 down to 1650 @ 150 degrees per hour.  Good luck.

That would be great, when are you coming???  Thanks a ton Tracy, I will let you know how it turns out.  I have a firing in about a week.  I will try to make you proud.....

After the hold to 1650 for an hour do you do and slow cooling?  If so, can I have your firing schedule?

Tracy Shea said:

I'm with Randy on the hold at 1650 for an hour.
This is a red glaze I use, almost identical to "Randy's Red"- got it years
ago in school.


flint-26
epk-4
RIO-18
Gerstley Borate-28 (I still have a stash, haven't subbed yet.)
F4 spar-18
talc-12


M^6 "Waterfall Brown" will also turn red if you fire this way.

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service