John Britt's Snowflake Crackle - The cone 6 oxidation glazes

John had a great article in the Nov. 2011 issue of Ceramics Monthly which was excerpted and republished on the Ceramic Arts Daily Website as "Crazy Beautiful Crazing: Uncovering the mysteries of Snowflake Crackle Glazes" Click Here to go to the online article. I contacted John Britt and he said it was OK to reprint the recipes here so our interested members can carry the conversation forward.

Here are the recipes.

Recipe Name:  Original Snowflake Crackle
Cone:  6/7     Color:  Translucent     Firing:  Oxidation     Surface:  Glossy

Amount     Ingredient

  4.26          Magnesium Carbonate

 89.36          Nepheline Syenite

  6.38          Ball Clay--Old Mine #4
100         Total

Additives

2.00          Bentonite 

The glazes seem to work best on dark brown bodies.  Use only small amounts of colorants, as a lot will kill the crazing.

 

Recipe Name:  Snowflake Crackle #4
Cone:  6/7     Color:  Translucent    Firing:  Oxidation     Surface:  Glossy

Amount     Ingredient

   7.86 Talc

   5.77 Ferro Frit 3124

 86.37 Nepheline Syenite

100 Total

Additives

   2.00 Bentonite

   0.20 Copper carbonate for Turquoise

 

Recipe Name:  Snowflake Crackle #8
Cone:  6/7     Color:  Translucent    Firing:  Oxidation     Surface:  Glossy

Amount     Ingredient

   3.94 Magnesium Carbonate

   7.41 Ferro Frit 3124

  82.74 Nepheline Syenite

   5.91 Ball Clay--Old Mine #4

100 Total

Additives

   2.00 Bentonite

   0.20 Copper carb for turquoise

   0.50 Superpax for white

   0.066 Cobalt carbonate for blue

   0.50 Degussa stain 239416 for yellow

   0.50 Red iron oxide for rust red

 

Views: 15309

Reply to This

Replies to This Discussion

Thanks! I will keep testing. I will see what I can get in the broad area I call local and will post results. I think you are right about the clay. I was very careful with the bisque fire.

Norm Stuart said:

I can't guarantee we've tried Snowflake with all of these clays, but these are our combined clay orders over the past five years.

WC 371 Big Pot Clay 60 mesh sand
WC 373 Dark Brown Clay -- fine sand
WC 376 L.B. Blend Clay 60 mesh sand
WC 381 Big White Clay with grog & sand
WC 384 Dave's Porcelain
WC 398 WS-4 gray/white with fine sand
WC 429 RSMC Red Clay
WC 894 Half & Half SC
WC-353 Paper Clay Cone 10
WC-370 Amador Cone 10 - densifies nicely at Cone 6
WC-390 Laguna Red
WC-391 B-3 Brown Black
WC-395 Porcelain Five
WC-400 Morrocan Sand
WC-402 Half n Half - pinholes with Ferro 5301
WC-412 Stoney White - new
WC-423 Greystone - contains magnesium or zinc which turns some blue and green glazes brown
WC-436 B Mix 5 with Grog
WC-438 Red B-Mix with grog   Easy Dry
WC-841 Danish White Clay
WC-842 Danish White Clay -- fine sand
WC-851 52 Buff
WC-861 Haggi Porcelain
WC-866 Electric Brown
WC-886 B Mix with Grog Paper - extremely problematic blistering, order only WC-353

Penny Berglund said:

I will try another clay body. I will also ask my supplier what they think. I am getting good crackle even where it is thin which would mean I won't have to go so nuts with the thicker glaze layer.

Is there a Laguna clay body that has worked for you with this glaze? IMCO? I can get clay at Clay Art Center in Tacoma, and I will be in Seattle next week and can get the clay bodies that Seattle Pottery Supply makes up as well. Since I am in the gorge now, it is also possible to make a trip to Portland to try what Georgies makes up.

Penny

I contacted John Britt, and other than trying other clay bodies, he had no suggestions. I did find it interesting that the worst problems were on the outsides/undersides of the pieces. Any idea about why that would be?

Penny

Snowflake glazes, like high-magnesium crawl glazes, have a tendency to fall off ware before it's melted in places where gravity does not favor it remaining in place.

Fire a bowl upside-down and you'll most likely discover the snowflake glaze is fine on the outside of the bowl but the glaze coating is thin and spotty on the upside-down inside of the bowl.

I experience the same problem with two layer oil-spot glazes where you place a runny top coat over an iron-rich base glaze. But in this instance the runny top glaze slides off after it's melted. Gravity is one of those laws or something like that.

I will try this next test go round. It would make sense with the large bubbles I got at times. But it still doesn't explain the pinholes prevalent on the undersides of pieces that had an even glaze surface and no bubbled lava effects.

About that Snowflake crackle #4, I used that on several clay bodies and found I got a much better, more predictable result by spraying it on rather than dipping. It tends to settle very quickly and the talc/nepheline combo tends to clump when dipped.

Very nice finish when sprayed though.

Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service