Hi all,

I was working on my shopping list for the local ceramics supplies store and saw Copper Sulphate listed under coloring oxides.  It is a brilliant teal blue.  I have never seen this in a reciepe.  Has anyone else?  What did the resulting glaze look like?

Views: 2809

▶ Reply to This

Replies to This Discussion

If you are looking at novel materials, do this Google search for decomposition temperature or melting temperature.

http://www.google.com/#q=Copper+Sulphate+decomposition+temperature

or

http://www.google.com/#q=copper+sulfate+wiki

to get this page

http://en.wikipedia.org/wiki/Copper%28II%29_sulfate

This Wikipedia page (below) shows the blue hydrated version loses its water at 230 F to become the teal Anhydrous Copper Sulphate which then decomposes into Black Copper Oxide and Sulphur Trioxide gas at only 752 F (560 C), or Sulphur Dioxide depending on the conditions.

So you can see, working in ceramics, you're not going to have Copper Sulphate, but only Black Copper Oxide CuO.

So you might get lucky with this Google search 

http://www.google.com/#q=Digitalfire+copper+sulphate

http://www.google.com/#q=Digitalfire+black+copper+oxide

Which takes you to these pages

http://digitalfire.com/4sight/material/copper_sulfate_239.html

http://digitalfire.com/4sight/material/copper_oxide_black_237.html

Here's both pages side-by-side. (click on the photo to expand it to full size)

Digitalfire quickly tells you Copper Sulphate has only 31.85% as much Copper Oxide as Black Copper Oxide. The balance of the Teal Blue material burns-off in the kiln as sulphur trioxide gas listed as LOI = Loss on Ignition.

So the resulting glaze color will be exactly the same as if you had added 31.85% as much Black Copper Oxide — or 49.46% Copper Carbonate which comes from the Digitalfire page for Copper Carbonate.

You won't always find a decomposition temperature for every material, but instead will find the Melting Temperature and the Boiling temperature - and that's good news if the temperature listed is hotter than your kiln — it means it's a suitable glaze material.

Take the ceramic flux Lithium Fluoride as an example which melts at 1,553 F (about ^013) and boils at 3,049 F, well above Cone 11 which is only 2,294 F.

If you could get a kiln that hot, the Lithium Fluoride will quickly melt then boil — then condense back into liquid Lithium Fluoride as soon as it finds a place cooler than 3,049 F and crystallizes into a solid at 1,553 F.

http://en.wikipedia.org/wiki/Lithium_fluoride

Some potters are convinced Lithium Fluoride breaks down into Lithium and dangerous Fluorine gas, but the heat required for that is phenomenal, far, far hotter than the 3,049 F which makes it boil. A temperature so hot the number isn't even listed — and no one has a kiln that hot unless you have a research lab.

I have used Copper Sulphate in recipes for electric fired self-reduced reds.  The sulphate dissolves better in water and gives you a better looking red when using a really fine mesh of Silicon carbide.  Like Norm's numbers indicate, it is not even as strong as the carbonate, but you don't need a whole lot when working with self-reducing copper reds.  jhp

Thanks for the info guys.

I used copper sulfate in pit fires. Pour a solution of copper sulfate in water (1tbsp/2 cups) over your bisque ware before putting it in the pit and/or sprinkle copper sulfate powder over the wood in the pit. Results:  reddish spots.

Spraying copper sulfate solution on bisque under a clear glaze and fire cone 6ox gives a watery blue effect.

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service