I got this recipe from the art center I go to.

 

This does run some.

 

and it is figured out in grams for a pretty large batch. I will try to get the correct formulas in the simplified format

 

EPK-   1116

Flint-   780

frit 3134- 2010

Neph Sy - 1674

Cob Carb- 84

RIO - 222

 

I will get the formulas next time I am there.

Views: 1727

Attachments:

▶ Reply to This

Replies to This Discussion

EPK  20

Flint 14

Frit 3134  36

Neph Sy    30

 

+ 1.5%    Cobalt Carb.

+4%        RIO

BLUE HARE’S FUR/FLOATING BLUE

(RON ROY) ^6 Oxidation

47.3 Nepheline syenite

27.0 Gerstley borate 

20.3 Flint - silica

5.4   EPK

2.0   Red iron oxide

1.0   Cobalt carbonate

4.0   Rutile (milled)

A multi-phase glossy blue which is very stable.

This glaze should be either poured or dipped and slow cooled (as suggested in MC6 Glazes) for good color and crystal development. To create the Blue Hare’s version, use Cobalt Oxide instead of Carbonate to get the dark blue flecks.

 

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service