Recipe Name: Nutmeg Variation      from Randy McCall

Cone: 6 Color: red
Firing: Oxidation Surface: Glossy

Amount Ingredient
23.3 Dolomite
23.3 Spodumene--Gwalia
6.8 Frit--Ferro 3134
23.3 Red Art
23.3 Silica

100 Total

Additives
3.2 Yellow Ochre
4.9 Tin Oxide

Unity Oxide
.163 Li2O
.034 Na2O
.029 K2O
.35 MgO
.424 CaO
1.000 Total

.272 Al2O3
.061 B2O3
.03 Fe2O3

2.568 SiO2
.008 TiO2
.001 P2O5

9.4 Ratio
58 Exp

Comments: This is Burush Regular Nutmeg
Changed kaolin to red art and left off iron oxide


Stars
Comment by Vickie Wilkes on November 10, 2014 at 6:06am

This is a gorgeous pot.  Any chance I could get the recipe for the glaze?  Also, what part of TX are you in...I'm in Kerrville which makes it a little hard to get supplies. 


Stars
Comment by juli long on June 23, 2013 at 11:38am

Roberts, thanks for the kind words!!

juli


Stars
Comment by Robert Serva on June 23, 2013 at 7:55am

Very Nice, Color and carvings go well together.


Stars
Comment by juli long on June 23, 2013 at 7:52am

Randy McCall nutmeg variation on cinco rojo

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service