How much rutile to make a blue cone 6 glaze?

This is 2, 3, 4, 5% rutile added to an 80:20 mix of Alberta Slip and Frit 3134 at cone 6 (GA6-C recipe). I use the 4% often, very nice blue with zero expensive cobalt).

Views: 932

Comment

You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!

Join Electric Mid&Hi Fired Ceramics

Comment by Kathy Ransom on October 13, 2012 at 9:59am

This is a photo of Raven's Lime on a pot and I've put the recipe on Insight but if you don't have access I can add the recipe here if you're interested. http://cone6pots.ning.com/photo/dsc02383?commentId=2103784%3ACommen...

Comment by Tony Hansen on October 11, 2012 at 9:42pm
Comment by susan claysmith on October 11, 2012 at 9:06am

HI Kathy - This colours of this glaze on Plainsman M340 seems to range from Amber (where thin) to a powder-blue, while on the M370 it ranges from Amber to a purplish-powder-blue.  

You mentioned a Raven's Lime - what are you using as a colourant?

Comment by Kathy Ransom on October 11, 2012 at 6:02am

I checked out your mugs Susan and love the colour variation in them so will definitely be trying the Alberta slip recipe.  Quite a few of my favourite glazes have ravenscrag slip as their main ingredient Tony.  I find it very stable and even have a couple that will do funky things like raven's lime which gives me a great lime base and grey spots.  I'm working on that one to see if I can get it in more colours.

Comment by Tony Hansen on October 10, 2012 at 9:38pm

Note that each glaze at albertaslip.com has clear instructions. This particular glaze does not work nearly as well on porcelain as it does on other bodies.

Comment by Tony Hansen on October 10, 2012 at 9:37pm

http://albertaslip.com is the place to learn how to use this material. I cannot live without it and ravenscrag slip now (http://ravenscrag.com).

Comment by susan claysmith on October 10, 2012 at 6:45pm

I have used this glaze with 4% rutile on Plainsman M370

Here are two examples of finished pieces with 4% rutile, and as you can see there is a lot of colour variation depending on how thick the glaze is and how it pools.  It's a simple glaze with great results!  Thanks Tony!  Susan

http://cone6pots.ning.com/photo/mugs-multi?context=user

http://cone6pots.ning.com/photo/alberta-slip-blue-mugs-1?context=user

Comment by Kathy Ransom on October 10, 2012 at 7:21am

Thank you Tony, I'm going to try the one with 4% rutile especially as I really like the breaking brown.

Comment by juli long on October 8, 2012 at 4:44pm

Tony, does the alberta slip need to be calcined? I read where you talked about this and I have zero experience in mixing glazes so I hope you will chime in. please.

Juli

love the looks of this glaze and thought I might try it as my first glaze test.

Comment by Jan Wallace on October 8, 2012 at 2:37pm

Thanks for the great advice Tony!

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2025   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service