5-10 years ago I mixed up a bucket of Pete Pinnell's Weathered Bronze Green cone 6-7. It was fine years ago and produced just the look I wanted. This time the results were not good. The glaze is very matt and is Dark gray only. No green at all. I first suspected it may have been that I needed to be at cone 7 down rather than cone six down. As you can see in the photo  re-firing to cone 7 has not solved the problem. I'm now feeling that there has been a chemical change over the 5-10 year period. I can of course just mix up a new batch but then I would still not know what happened to the first old batch. I'd love to know why! Any educated guesses would be appreciated.

Recipe Name:  Pete's Weathered Bronze

Cone:  6-9     Color:  green bronze
Firing:  Oxidation     Surface:  Matte

Amount     Ingredient
60          Nepheline Syenite
20          Strontium Carbonate
1          Lithium Carbonate
10          Ball Clay--Old Mine #4
9          Silica

100         Total

               Additives
5          Copper Carbonate
5          Titanium Dioxide

Thanks

Otto Wenger 

Views: 1262

Reply to This

Replies to This Discussion

I found the same to be true, my older batch of Weathered Bronze no longer fires with any green in it so I went to the recipe below instead which seems to work even though it was mixed years ago.

STRONTIUM TURQUOISE MATTE ^5/6

The ingredients in this glaze are the same as the ones in Strontium Weathered Bronze; only the amounts vary slightly.  A beautiful matte turquoise glaze!
60% Nepheline Syenite
25% Strontium Carbonate
02% Lithium Carbonate
04% EPK
09% Silica 325
ADD:
04% Copper Carbonate
02% Bentonite


Barbara,

By eliminating Titanium Dioxide I think you have found the cause of "Weathered Bronze Green" interacting badly with some clays to create a mustard or ugly brown color. I'm going to mix up a batch of your recipe this Saturday and will post the results.

Titanium dioxide does not work like zircopax to provide a white background.

I once tried covering a darker clay with wash of titanium oxide, imagining I was covering a dark canvas with a ceramic guesso - boy was that a mistake!  I got the same bubbly brown covering seen in Otto Wenger's container above.

The nepheline syenite in Weathered Bronze Green will leech salts over time after being mixed with water which will cause the glaze to hard-pan leaving you to apply only some of the components of the glaze. Weathered Bronze Green also began llife as a Cone 10 glaze which means it's under-fluxed for Cone 6.  But I think in eliminating the Titanium Dioxide you've found the real problem.

Thanks to both of you for your insights. I have learned something and that was the goal. I will toss the old and give the new a try. I will post my results. Looking forward to seeing your results Norm.

Thanks

Otto

Normally I'd use a gram of water for a gram of glaze but the Strontium Turquoise Matte has so little clay it tolerates less than half the water. Initially using more water the glaze wouldn't apply except on extremely porous bisques.

I made a strontium version and a barium version. It will probably be three weeks before the test tiles are fired, as "folks are working on the kiln".

I made Barbara's Strontium Turquoise Matte on the LEFT fired on four different clays.

and I replaced the Strontium with Barium on the RIGHT.

It's a typical Barium Blue as the Strontium or Barium shift the green color to blue, but not even close to a Weathered Bronze Green. Her recipe uses 25% strontium carbonate rather than 20% and leaves out the Titanium Dioxide.

I would suggest you add 20% Ferro 3269 Frit to the Weathered Bronze Green, which is my variation to make sure this Cone 10 glaze recipe melts fully at Cone 5/6.  I doubt the results were changed by aging, but a reaction with the type of clay.

What happens if you leave the lithium out

Lithium Carbonate or Lithium Fluoride are fluxes which make glazes runny. As a color, lithium contributes only a clear glass.

If you leave out the lithium, you have to replace it with more of another flux material like the nepheline syenite or the Ferro Frit 3269 which I add to my version of the glaze to be certain it melts at Cone 6.

The fluorine in the 3269 or in the Lithium Fluoride can add white whisps to the flow of the glaze.

Water Color Green has many of the same ingredients, lithium, copper, calcium carbonate, and strontium carbonate.  But it's missing the Ball Clay, titanium, and Nepheline Syenite Both lithium and Strontium color-shift copper to a bluish tint by making the molten glaze more alkaline.

108.2% Water Color Green ^6
48.0% Feldspar Custer
17.0% Silica
16.0% Whiting
7.0% Strontium Carbonate
5.0% Ferro Frit 3124 or change to 3269
4.0% Lithium Carbonate
3.0% Bentonite
8.2% Copper Carbonate
3.0% Magnesium Carbonate

Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service