Potters & Sculptors - Making Rock from Mud
I am testing my various porcelains, I'm using tried and true recipes that I have used before. I checked my cones and they are showing 6 fully down and 7 just starting to bend at the tip. I have used these glazes on at least some of these clays before with no problem.
Firing is a slow warm up and controlled cool with a 30 min hold at max temp.
The only thing I have changed is that I now bisque at cone 08 instead of 04 could this being causing some of my glossy glazes to come out Matt?
Any advice would be greatly appreciated, I so miss my shiny Amber.....sigh
Tags:
A controlled-cooling will result in more glaze crystallization and a more matte result. I would guess you haven't previously slow-cooled these glazes.
If slow-cooling not your problem I'd like to see the glaze recipes and photos of the glazes, before and now.
Glazes which turn matte with a slow-cool can be made glossy with a slow-cool by adding more flux and glass. Adding 50% Ferro Frit 3269 can make almost anything glossy, even though it may not necessarily look like the original glaze.
As an example, this is Pete Pinnell's Weathered Bronze Green, intended to look very matte like the photo on the left. The right-hand photo has 50% 3269 added, and is clearly glossy at slow-cooling, even though it looks nothing like the original.
If your bisque firing is fairly slow, most bisque gas generation will be finished half-way between ^07 and ^08, but immature bisque would be producing pin holes rather than a matte glaze.
Thanks Norm
This would make sense as I never did a slow cool before the last two firings and that is when I noticed the change in my glazes. I will do another firing and eliminate the slow cool or maybe just speed it up a bit. Below is what I did last firing, it's a slightly altered Steven Hill schedule. I wanted to try it to see if I would get something more from my existing glaze palette.
1 200 deg/hr to 220 hold 1 to 3 hrs depending on wetness and thickness
2 100 deg/hr to 500
3 400 deg/hr to 2100
4 100 deg/hr to 2160 hold for 1 hr
5 9999 deg/hr to 1700
6 50 deg/hr to 1600 hold 30min
7 50deg/hr to 1500 no hold kiln off
Brenda
Norm Stuart said:
A controlled-cooling will result in more glaze crystallization and a more matte result. I would guess you haven't previously slow-cooled these glazes.
If slow-cooling not your problem I'd like to see the glaze recipes and photos of the glazes, before and now.
Glazes which turn matte with a slow-cool can be made glossy with a slow-cool by adding more flux and glass. Adding about 50% Ferro Frit 3269 can make almost anything glossy, even though it may not necessarily look like the original glaze.
As an example, this is Pete Pinnell's Weathered Bronze Green, intended to look very matte like the photo on the left. The right-hand photo has 50% 3269 added, and is clearly glossy at slow-cooling, even though it looks nothing like the original.
If your bisque firing is fairly slow, most bisque gas generation will be finished half-way between ^07 and ^08, but immature bisque would be producing pin holes rather than a matte glaze.
This is Ron Roy's Sapphire Blue, with increasingly slow-cooling, which is typical of the changes you'll see.
Controlled-cooling emulates a cone 10 gas kiln because the hard fire-brick of a gas kiln retains heat and cools very slowly. The result is often more sophisticated, and sometimes disappointing.
Clear Base Blue (below) was a glaze which needed some extra frit to become a beautiful glaze at slow-cool.
I think Fluorine is an under-appreciated flux because of overblown concerns about free HF gas. Ferro Frit 3269, 5301 and Cryolite are great ways to free up a glaze which becomes over-crystallized with a slow-cool.
Sorry Norm I don't have a pic of the glaze as it was when I saw it, it's new to me but I have seen it glossy.
The other is a Jade recipe that I layer over another that usually comes out very glossy.
Feldspar- Custer 40
frit Ferro 3124 9
Whiting 16
Talc 9
EPK 12
Silica 16
Add: Copper Carb 5
Rutile 6
This is the old firing of Jade over my Cream Brulee glaze
This the Jade on it's own that I just fired
I haven't spent the time to think through why this is . . ., but as a general rule glazes with a big percentage of Nepheline Syenite don't often produce a beautiful glaze with a slow-cool, without adjustments to the glaze recipe.
Low-temperature melters like Gerstley Borate or frit don't produce the sort of problems Nepheline Syenite does with slow-cooling.
The 7% rutile you're adding, is close to enough titanium dioxide to matte most glazes. Titanium matte glazes use 8% to 16% titanium dioxide. Slow-cooling will increase the titanium crystallization.
Slow-cooling Pete Pinnell's "Weathered Bronze Green" also brings out a mustard color and diminishes the green.
This is the original recipe for Weathered Bronze Green,
60 Nepheline Syenite
20 Strontium Carbonate
10 Ball Clay
9 Silica
1 Lithium Carbonate
5 Copper Carbonate
5 Titanium Dioxide
This is my revised recipe for slow-cooling at 50 F per hour between 1800 F and 1500 F
This is Alisa Clausen's tile of Weathered Bronze Green, showing one of the many ways this glaze can go wrong.
It is a ^10 recipe used at ^6 without adjustments.
Adding the additional 3269 frit helps, as does replacing the Lithium Carbonate with Lithium Fluoride. Like any ^10 glaze it needs more flux to become a reliable ^6 glaze.
Does it have to be 3269? and I don't have any Lithium Fluoride. I have to laugh, just when I think I have every glaze chemical I will ever need I find out that I don't.
Hey Norm
Where do you get Lithium Fluoride? I just checked the Clay Art and Seattle Pottery catalogues and couldn't find it.
Lithium Fluoride is a relatively new raw material for art ceramics, being distributed by Laguna Clay and their Axner subsidiary.
http://www.axner.com/lithium-fluoride.aspx
It costs more than lithium carbonate but I like it a lot.
If I didn't have access to lithium fluoride I'd be using Cryolite or Ferro Frit 5301 in addition to the lithium carbonate. Lithium fluoride is ever so slightly more "fluxy" than lithium carbonate, but the flow patterns it creates in the glaze are typical of fluorine - you don't get that with lithium carbonate alone.
Ferro Frit 3134 or 3110 can be used to add more glass to a glaze that over-crystallizes with a slow-cool. But Ferro Frit 3269 is fairly fluxy having 1.6% Fluorine in addition to potassium and sodium, while 5301 has 9% fluorine in addition to the potassium and sodium, so even fluxier still.
http://digitalfire.com/4sight/material/ferro_frit_5301_468.html
http://digitalfire.com/4sight/material/ferro_frit_3269_371.html
At $3 a pound Cryolite is probably the cheapest was to buy fluorine flux.
http://www.axner.com/cryolite.aspx
http://digitalfire.com/4sight/material/cryolite_250.html
The drawback to 3110 frit is it adds the sodium, thus increase glaze expansion and crackling/crazing, without adding a lot of other flux so you have to add relatively more of it.
This is an example of what fluorine adds. These are tiles of Magruder Red made with impure and relatively brown Laguna Red Iron Oxide.
The first tile is Magruder Red with 10% Ferro Frit 3134 added.
This second Magruder Red has 10% Ferro Frit 5301 added - notice the metallic crystal sparkles.
This tile is Magruder Red, but made with synthetic Red Iron Oxide.
Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase
Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com
Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.
Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.
The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.
Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .
If you are up to creating videos of your work or techniques you might want to invest in a flip video camera
Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00
And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62
ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.
If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014
© 2025 Created by Andrea Wolf. Powered by