"I'm having trouble with a lovely glaze I used before; I have a lot of pin holes , I refired the plates at a slightly higher temperature 1260°c instead of 1240°c, soaking it longer (30 mns)too but no changes ! I checked and I do have pin holes even with another clay body .
Here's my recipe :
Potash Feldspar 54
Dolomite 18
Quartz 18 
Kaolin 5
Rutile 5
+
Copper Carbonate 1
cobalt carbonate 1

Someone mentionned "salvation glaze" might help ...any information on that ? how could it help ? what's the recipe ?

I'm in France so I translated my "ingredients" but can't give any more references ..

Thank you Evelyne

Views: 838

Reply to This

Replies to This Discussion

Hi Evelyne,

      I have used this before & it has worked for me.

Salvation Glaze ^6

This recipe was in a pottery magazine a couple of years back and it’s great to fix problems…crazing…blisters, etc.  It WILL change the color of the original glaze, but wow it’s pretty and will fix most problems.

Custer spar              27.0

Gertsley Borate        21.0

Dolomite                      8.8

Talc                           19.5

OM4                            7.5

Silica                           25.2

Cobalt Carb                  3.0

    Mix some up & apply it to your pot that has been heated in the kiln or oven.  Keep the heat at around 100 C. so you don't crack your pot when applying.

When people in our studio have pinholes in a ceramic fired to ^6,  I tell them to apply a ^06 glaze and fire again to this lower temperature 998C.

The higher percentage of "flux" (fondant pour céramique) in the ^06 glaze mends the surface of the ^6 glaze. I have never seen a ceramic already fired to ^6 give off additional gas at ^06.

"Salvation Glaze" for pinholes at ^10 is a similar concept. It is a very liquid glaze which mends the pinholes.

http://www.potters.org/subject103651.htm

I will make your glaze to see if I get pinholes at 1222C. I don't know enough chemistry to tell you what is causing the gas after soaking it for 30 minutes. I assume an interaction between the glaze and clay.

I do not know enough chemistry to tell you what is causing the gas after soaking for 30 minutes.

XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX

Quand les gens dans notre studio ont piqûres dans une céramique cuite à 6 ^, je leur dis d'appliquer un ^ 06 glaçure et tirer à nouveau à 998C.

L'augmentation du pourcentage de "flux" (écoulement fondant céramique) dans le ^ 06 glaçure répare la surface de l'émail ^ 6. Je n'ai jamais vu une céramique déjà tiré à 6 ^ dégagent du gaz supplémentaire à ^ 06.

Salvation Glaze trous d'épingle à ^ 10 est un concept similaire. C'est un vernis très liquide qui répare les trous.

http://www.potters.org/subject103651.htm

Je vais faire votre céramique-glaçure pour voir si ont piqûres dans céramique à 1222C.

Je ne connais pas assez la chimie de vous dire quelle est la cause du gaz après avoir fait tremper pendant 30 minutes. Je suppose une interaction entre le glaçure et l'argile.


Vous pouvez également remarquer que je n'ai pas assez étudié la langue française.

I tried your glaze on several clays, with different oxides. They were fired to ^6, with a 30 minute hold, followed by a slow-cool of 28 degrees C between 982 C and 815 C, a six hour period for this temperature range for glaze crystallization.

On the tile below I can see the tiny remains of two pinholes in the top of the tile, where there are 3 coats of glaze. If you use "dark rutile" which is not pre-calcined to remove gas producing components there will be more pin-holes. I used "light rutile" which is calcined.

This variation of your glaze used 1% cobalt carbonate instead of 3%, and 1% copper carbonate.  The original 3% cobalt carbonate did not pinhole at all.

Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service