So im more of a figuative sculptor but am having trouble finding a cone 6 base flesh tone recipe. Anyone have any suggestions?

Views: 312

Reply to This

Replies to This Discussion

Rutile Matte - This is the skin tone of my Clayton Mudd character.
Cone: 6 Color: pinkish orange
Firing: Oxidation
Surface: Slightly variegated matte
I don't recall the source of this recipe
Amount Ingredient
44    Nepheline Syenite
17.4 Whiting
14    Kaolin--EPK
19.6 Silica
5     Zinc Oxide

Additives
7     Rutile

This might not be exactly what you're looking for, but it might be a good starting point where you can vary the amount of rutile and/or other colorants such as iron or manganese. As a plus, it has been very consistent and reliable for me.  Good luck.

This is a little off the point, but I always thought it was sort of funny. First I want to say that I am a very unprejudice person and I don't want any of this to be taken wrongly. I am quite white and at one point in my life I was dating a black gal.  Great gal. We went by my moms chuch for some reason and when we got there my mom had just finished painting the nursery area. The color was the old stand by "tenement pink"  ( almost as bad as "Landlord Green") Mom says " We painted this flesh tone." My girlfriend laughs and says  "Whos flesh?" There is probably no point to this blog but I can't hear the words flesh tone and not smile a bit.... I do have a caucasian glaze. How I came by it may throw you for a loop... They say necessity is the mother of invention. I think poverty is much more maternal. I did a mural for a lady wanting her childs portrait on an  illustration from the book "the Velveteen Rabbit" To get the flesh tones for the little girl I used some glaze that had given to me. The brand is A.R.T.  wwwartclay.com I do not know if they are still around. I used a mix of Bone FW2045 and Blush FW2042 . I used a rato of 3/6, 6/6, 6/3 of the two glazes for a contrast of light and dark. I fired them to cone 6,  flat. This was a tile piece. They came out perfect. The loop? They are lowfire 05 glazes. If I need a caucasian face glaze again, this is what I will use. I myself need a glaze for five African children faces "Flesh tone" I worked on one for a long time and it is sort of so so. Skin tones are hard. Talking too much, Kabe

My little man there is definitely in a minority of existent flesh tones. What's really embarrassing is that I didn't even think about it. Thanks for the wake-up call, Kabe. 

Hi George, No reason to be embarrassed The whole conversation was a "Ah-ha" moment for me at the time. I am looking for a picture of the mural I think it is on some slide film. I am going to run some test tiles of the 05 glaze fired at cone 6 to show how will it worked. I hope it will again. Plus I really do need a good flesh tone for the faces of 5 African children. Have a great day

Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service