Hello everyone,

I am trying to find a recipe for a crystalline glaze with small but well-visable cristals for c.6

Prefeable without barium.

Is there anyone who has a recipe for me?

greetings,

marlies

Views: 2123

▶ Reply to This

Replies to This Discussion

i don't know the digitfire format yet, but as percentages and off the top of my head a good reliable crystalline glaze is:

3110 frit  50

silica       23

zinc oxide  23

titanium   1-3  

lithium carbide  1-3

then add colorants -- cobalt, copper, nickle, iron, manganese are all good

You will need something to keep it all in suspension like CMC gum or a little bentonite (sp?)

But the the real trick with crystallines is the firing schedule  up to 2130F then drop to between 2000-1800 , go up and down in there - then fall off slowly to 1400F -- ya kinda gotta find your own way

Oh! then the real fun comes chipping it off it's base -- use a pedestal and glaze catcher, made to fit and hopefully you can get it unstuck with a blow torch if ya used the right glue to hold it together up front -- there's a lot to it and I've trashed a few pieces of furniture as I've learned and figured it all out.  Good luck!

i gotta get my act together on the computer, arrg

Attachments:

oh! and one more thing, the pictures are mislabeled, the one is nickle and the other cobalt.. sigh -- i'll figure it out yet  -- the lithium is what brings the recipe down from a a cone 10 to a cone 6

Hi Steve,

thanks for your reaction. The pictires look great, a pitty the yellow one broke!

i am going to try your recipe.

greetings,

marlies

put it on thick too, especially up top, it will run a lot  , and long soaks, i just got to the top temp and drop, but then sit at 2000  a couple hours, and at each spot 1950 an hour maybe, 1975 an hour, 1925 an hour.. 1900 ... that kind of thing --- do a search there are a lot of good sites out there -- the glaze i gave is kinda a basic forgiving one -- good luck

I have better pictures and a half completed website, i have to figure it all out, but i want to do my next firing first!

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service