Penland Red-Orange posted by Michele Hartung 6/29/2011   

Feldspar, F-4       46.70 

Talc         16.90 

Bone Ash     15.00 

Crocus Martis      11.50 

Silica         11.40 

Kaolin, EPK           4.00 

Lithium Carb         4.00 

Bentonite             2.00
                    111.50

Comment by Michele Hartung on July 27, 2011 at 3:44pm. This is without reduction.  It is Penland Red-Orange on Highwaters Loafers Glory clay.  It is dipped in "thick" glaze (or dipped twice in a thinner version)  and given a 30 minute soak at peak, cone 6.  Ends up at cone 7.  If you are going to try this glaze, layer it on very thickly, otherwise you get brown.


Views: 5119

▶ Reply to This

Replies to This Discussion

Fantastic, I tried it and will post pic.  I also made a small test batch using yellow crocus - that came out really nice, I'll post pictures very soon.

 

Hi Jette, what color did the yellow crocus produce?  Do you have any pics yet?

Have not had time to take pictures, I'll post them as soon as I have time.  Pretty silly but right now I can't even remember what color I got..I am loosing it.

 

I mixed it up and I'm trying it. Hope it looks as gorgeous as what you've got goin' there. 

I would like to try this glaze. Where do you get your crocus martis?

Mid-South ceramics in Nashville, Tennessee, although you can probably find it at a dealer near you!

Thanks, DJ.  Remember, it has to be thick, otherwise it is brown.  Also, thin it out at the bottom or else you'll be scraping your shelves.  I usually dip for 4-5 seconds on the top and 2-3 seconds on the bottom.

neither of my usual suppliers carry it. I'll have to be a bit more resourceful.

Michele - Mid-South Ceramics doesn't currently list "Crocus Martis".  It would be wonderful if they gave you an MSDS for what they sold you.

The MSDS (Material Safety Disclosure Sheet) will essentially tell us what commercial red pigment Mid-South sold you as "Crocus Martis". I'm convinced using the correct product is the key to producing the right red color.

Michele Hartung said:

Mid-South ceramics in Nashville, Tennessee, although you can probably find it at a dealer near you!

You can get it from:
http://ceramicsupplyinc.com/chemicals.aspx
Norm Stuart said:

Michele - Mid-South Ceramics doesn't currently list "Crocus Martis".  It would be wonderful if they gave you an MSDS for what they sold you.

The MSDS (Material Safety Disclosure Sheet) will essentially tell us what commercial red pigment Mid-South sold you as "Crocus Martis". I'm convinced using the correct product is the key to producing the right red color.

Michele Hartung said:

Mid-South ceramics in Nashville, Tennessee, although you can probably find it at a dealer near you!

you can get from:http://ceramicsupplyinc.com/chemicals.aspx



Shine Chisholm said:

neither of my usual suppliers carry it. I'll have to be a bit more resourceful.

I was able to special order it. Thank you.

Jette Nielsen said:

you can get from:http://ceramicsupplyinc.com/chemicals.aspx



Shine Chisholm said:

neither of my usual suppliers carry it. I'll have to be a bit more resourceful.

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service