The best kiln wash I've used is from Ceramics Art Daily. It's more convenient than 1/4" of alumina hydrate powder on the shelf, but we currently use both.
Kiln wash containing Silica will melt if too much liquid glaze flows onto it.
http://ceramicartsdaily.org/firing-techniques/soda-firing/the-many-...
50% Alumina Hydrate
35% Calcined EPK Kaolin (sold as Glomax, or calcine your own in your kiln)
14% EPK Kaolin
1% Feldspar
1% Darvan 811 (deflocculates wash for self-leveling attributes)
As the article mentions, you need at least 10% to 15% kaolin to suspend the kiln wash. Glomax does not suspend but it also does not shrink. The 1% to 2% feldspar provides just enough melting to keep the kiln wash on the shelf, rather than powdering off.
The only space-age ingredient I can imagine Lee could add to kiln wash would be Boron Nitride, unless you consider Glomax to be a space-age ingredient.
Boron Nitride powder costs about $65 a pound and is also available in a spray can (used for glass molds). Boron nitride, like alumina hydrate, makes an excellent dry lubricant to allow heavy pieces to expand and contract in the kiln. The alternative is to use one fixed point and two ceramic pie balls (normally used to weigh down pie dough) to support a large piece in the kiln.
I've never compared boron nitride to alumina hydrate as alumina hydrate costs less than $2 a pound, but if I bought some it might surprise me. Oddly it's also used in most lipsticks and other cosmetics due to it ability to lubricate.
http://sandblastingabrasives.com/Bullet-Lube-Gun-Barrel-Bore-and-Bu...
http://www.amazon.com/Spray-Mold-Release-new-Nitride-Brands/dp/B00A...
http://digitalfire.com/4sight/material/boron_nitride_133.html
Add silica to stiffen without changing the finished look of a glaze, or a combination of silica with kaolin to maintain the ratio between silica and alumina.
I've found 20% added silica can make most low-fire ^06 glazes into successful ^6 glazes. Stiffening a runny ^6 glaze may take as little as 5% added silica.
If the glaze is made with frit or feldspars you can also reduce these somewhat to stiffen the glaze, but this will often change the finished look.
Norm, I use "Lee's super incredible kiln wash" and it is what it states. I just wish I knew what to add or take away from the glaze recipe to stiffen it up. Im not that glaze savvy!
Those extra feet are sadly a common occurrence at our studio.
As a result we've resorted to covering our kiln shelves with 1/4" of Alumina Hydrate "sand" on top of each kiln-washed shelf. That way the extra glaze sticks to nothing other than the ware it came from. For us it's an ideal solution.
Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase
Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com
Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.
Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.
The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.
Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .
If you are up to creating videos of your work or techniques you might want to invest in a flip video camera
Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00
And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62
ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.
If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014
© 2026 Created by Andrea Wolf.
Powered by
You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!
Join Electric Mid&Hi Fired Ceramics