This a flow tester fired at cone 6. On the right is G1214W, a typical cone 6 transparent fluxed by a boron frit (google it). On the left is typical of what many use to achieve a matte. The recipe is: Nepheline Syenite 40, Dolomite 15, Whiting 10, Ball Clay 20, China Clay 10, Silica 5.

This simple comparison teaches us many things about glazes and even ourselves. Here are some of them.

-Cone 6 glazes require boron (from frits or gerstley borate) or zinc to melt (the one on the left has neither). Materials like feldspar, dolomite, whiting and talc just do not melt well at all at cone 6. If a glaze is not properly melted then it is not hard and strong and resistant to leaching and cutlery marking.
-Textbook glaze recipes often are junk. Unquestioned use of them demonstrates our willingness to accept something ridiculous just because it is in a book or on a web page. We need use common sense when looking at glaze recipes for cone 6 to determine if they are for real or impostors (the glaze on the left is actually really not a glaze, it is a porcelain). If there is no frit, no zinc, no gerstley borate, then a red this-likely-does-not-melt light is flashing.
-Glazes with high feldspar or nepheline syenite (40% is really high) are likely to craze. If this one does not craze it is simply because it has not melt enough for the sodium to impose its high thermal expansion on the glass.
-A cone 6 glaze with 30% clay (in this case ball clay and kaolin) and no boron is certainly not going to melt well because clay is refractory.
-True matte glazes have high alumina and low silica (which this has) but they also need to melt well to form a glass (which this does not). So this is just a matte because it is not melted.
-If a white-firing glaze has no zircon or tin oxide, then how can it be white? Something is wrong. In this case it is white simply because it is not melted.
-Since this does not melt, evaluating it on the basis of its chemistry would be invalid. Ceramic chemistry theory depends on the glaze being melted to a homogeneous glass. Thus, in addition to knowing all about the chemistry, you need to have common sense on the recipe level also.

Views: 123

Comment

You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!

Join Electric Mid&Hi Fired Ceramics


Stars
Comment by Jan Wallace on November 19, 2012 at 11:36am

Excellent information Tony. Thanks. :)


Stars
Comment by Kabe Burleson on October 24, 2012 at 5:24pm

Still learning here. Does the G1214W refer to the glaze as it is listed in Insight-live or is there somewhere else I need to look. Thanks

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service