The pink must be Tin reacting with the 23.1% Boric Acid in the frit.

Powder Box Pink
50.0% Ferro Frit 3134
25.0% Silica
15.0% Ball Clay OM4
7.0% Tin Oxide
5.0% Calcium Carbonate

http://www.potters.org/subject00170.htm

Views: 119

Comment

You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!

Join Electric Mid&Hi Fired Ceramics


Stars
Comment by Norm Stuart on May 31, 2013 at 1:01pm

The glaze is very hard and glassy but melts well, as you'd expect with a glaze coupling 50% 3134 frit with clay and silica. The thermal expansion is 6.74 with a Silica/Boron:Alumina ratio of 32.

I'm going to try the Powder Box Pink with 5% and 10% more silica to make the glaze more refractory and reduce the flow.

This was fired with a six hour slow-cool between 1,800F and 1,500F. So it could look different fired differently, or it could look the same.

This is the book it allegedly was taken from. (An earlier edition)

http://www.amazon.com/Out-Earth-into-Fire-Materials/dp/1574980785


Stars
Comment by Denice E. Demuth on May 31, 2013 at 12:48pm

Very interesting, is it a stable glaze?  Denice 

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service