I will share what I know about this glaze. I started with a base white glaze that I found in a CM 11-1989 on page 36. It says that it is cone 6-8 but I found that it can get pretty fluid at cone 6. I tested about 20 different oxide combinations and this is my favorite.
Dolomite 19.48
Gerstley Borate 12.99 the real stuff!
Kona F-4 38.96
Flint 28.57
Zinc Oxide 12.99
ADD
Titanium Dioxide 10 percent
Black Iron Oxide 2.5 percent
Copper Carbonate 5 percent
If any of you give it a try please let me see how it works out for you.
That is a really nice glaze.
Troy I just love a glaze that you can just fire no ramping up and down and it comes out perfect every time. Denice
Wow this is beautiful!!!! Is this your own recipe?
Yes, it's a cone 6 without any fancy holding or cooling cycle.
Oh wow. I love it. Very pretty. Is it a cone 6 glaze Troy?
Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase
Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com
Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.
Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.
The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.
Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .
If you are up to creating videos of your work or techniques you might want to invest in a flip video camera
Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00
And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62
ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.
If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014
© 2024 Created by Andrea Wolf. Powered by
You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!
Join Electric Mid&Hi Fired Ceramics