Potters & Sculptors - Making Rock from Mud
These are some different mason stains in the cone 6 transparent G1215U glaze. Google 'G1215U' for the recipe, it is very good on porcelains but has an MgO containing frit which is more expensive (but worth every penny). It was formulated to be very low expansion, so it not only is less likely to craze, but is adjustable.
Tags:
Comment
I made G1215U yesterday and tried a batch with 3% Magnesium Carbonate added, which increases the magnesium in the glaze by 53% from 2.4% to 3.7%. The extra Magnesium makes the glaze really silky, smooth and just a little glossier.
It costs more but, as you say it's worth it. Looking at the two glazes with a variety of Mason Satins
today, people at our studio were oohing and ahhing over the G1215U with the added MgCO3.
I also made some G1215U using Ferro Frit 3124, instead of 3249, yesterday which is less shiny but also makes a nice base for Mason Stains with a stiffer melt which covers better on texture and edges. But not as popular as the G1215U with extra magnesium carbonate.
It's just like the fact that our most popular glazes are those containing tin oxide, which is also expensive at $26 a pound. The more tin a glaze has the more people like it, even though many are really just variations of another. Glazes like:
Bailey Shino, 5% tin oxide;
Cream Breaking Rust, 13% tin oxide;
Heidi's Eggshell, 9% tin oxide;
Metallic (Green, Ocean Blue, and Sky Blue), 6.8% tin oxide;
Ron Roy Nutmeg, 4.85% tin oxide;
Spotted Aqua Brown, 2.9%;
Warm Jade, 5% tin oxide;
White Bird, 6% tin oxide.
Bailey Shino
Cream Breaking Rust
Warm Jade
White Bird
Magnesium does give that nice satin glaze surface.
What was the Mason Stain name for 6139? It looks like 6392 Dusty Lavender.
Is your yellow 6344, actually 6433 which was replaced with 6450 Praseodymium Yellow?
Nice colour response.
Hi Tony - I have lots of frit 3134 and no Frit 3249, but I am seeing some crazing on plates, so switching to G1215U sounds like the thing to do. Thanks for the feedback and advice - much appreciated, Susan
Why not use the G1215U recipe instead, it is better for porcelains. Check here: http://digitalfire.com/4sight/recipes/low_expansion_glossy_clear_co...
http://digitalfire.com/4sight/education/bringing_out_the_big_guns_i...
Thanks for this Tony! Thanks for posting this. I am currently using the G1412W on Plainsman M370, but am wondering if this will give me a better fit. Any thoughts? I will test it out next glaze firing. Susan
Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase
Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com
Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.
Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.
The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.
Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .
If you are up to creating videos of your work or techniques you might want to invest in a flip video camera
Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00
And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62
ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.
If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014
© 2025 Created by Andrea Wolf.
Powered by
You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!
Join Electric Mid&Hi Fired Ceramics