Nutmeg, Pavarotti Gold, and Licorice at the rim on Little Loafers clay

Views: 141

Comment

You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!

Join Electric Mid&Hi Fired Ceramics


Stars
Comment by juli long on August 14, 2014 at 6:31am

Thanks George for the info.  I had some Alberta slip on hand and not the Ravenscrag so I thought I would check.

I think the Pavarotti Gold is a nice glaze.

juli

Comment by George Lewter on August 13, 2014 at 8:36pm

Juli, it would be a very different glaze. As I understand it both Alberta Slip and Ravenscrag are produced by Plainsman Clay and their mineral contents are very different.

http://www.plainsmanclays.com/ravenscrag/index.php

http://www.plainsmanclays.com/albertaslip/index.php


Stars
Comment by juli long on August 13, 2014 at 8:09pm

George, 

Do you think the Pavarotti Gold glaze could be made with Alberta slip instead of the Ravenscrag slip?


Stars
Comment by Jeff Poulter on March 19, 2014 at 1:36pm

Hi George,

    Let's hope they're good!  I have liked the RS glazes I have done, especially the Plum Red.  I am going to try some Alberta Slip glazes as well.  I was also thinking of combining RS & AS, because you have to calcine 1/2 of the AS when you use it in recipes.  Will post some results, but I for sure want to try the PG layered.....  jhp

Comment by George Lewter on March 19, 2014 at 1:28pm

Jeff - Yes and Yes. The nutmeg they have down here is darker and matter than the way it comes out for me at home. I have used this combination along with Spearmint (from MC6G) with very nice results in my preliminary attempts. Three large bowls with these glazes sprayed on should be out of the kiln tomorrow. It may be a while before I can post photos, assuming they are worth posting :-) The Pavarotti Gold is a rich amber by itself over white clay. Based on results so far, I definitely want to try it layered with others of my stock glazes, and to take a longer look at the Ravenscrag Slip glazes in general.


Stars
Comment by Jeff Poulter on March 19, 2014 at 11:57am

Hey George,

     Is the PG layered over Nutmeg?  And is this the variation that you have listed below?  Looks good!  jhp

Comment by Lawrence Weathers on March 18, 2014 at 9:12pm

Thanks

Comment by George Lewter on March 18, 2014 at 5:12pm

Pavarotti Gold is the local name at MIY Ceramics and Glass for the Cone 6 base recipe for Ravenscrag Slip glaze (glossy), colored with red iron oxide.

Recipe

Material Amount
Ravenscrag Slip 80.00
Ferro Frit 3134 20.00
100.00


with additions of
6% Red Iron Oxide
2% Bentonite

Comment by Lawrence Weathers on March 18, 2014 at 4:37pm

what is what is Pavarotti Gold?

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service