Oil Spot Daly overcoat layered over raven's lime, fired to cone 6 in oxidation.

Views: 305

Albums: 2013

Comment

You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!

Join Electric Mid&Hi Fired Ceramics


Stars
Comment by Kathy Ransom on March 10, 2013 at 2:18pm

If you are a member of the Insight group both glazes are in that database.  The oil spot I used isn't Daly which is glossy black with tray spots (lovely) but this glaze which is meant to go over a glaze heavily laden in RIO.

Custer  20

Frit 3134  20

Wollastonite  15

EPK  20

Talc  6

Silica  19

Tin Oxide  4

CMC  2


Stars
Comment by Denice E. Demuth on March 9, 2013 at 9:01am

Thanks Kathy, I am going to be firing a load of Cone 6 in about a week and I could do some tests and throw them in. I have never had too good of luck with purchased glazes but do well mixing my own. Denice


Stars
Comment by Kathy Ransom on March 9, 2013 at 7:01am

Just searched the recipes on this network and on insight but ran into a glitch, likely caused by me so I'll try to fix and post or put a link to them shortly.


Stars
Comment by Kathy Ransom on March 9, 2013 at 6:33am

Thank you Denice :) The glazes I used are mixed up by me and I've been experimenting with layering. The first two layers were Raven's Lime and the last layer was the white overcoat of an oil spot glaze.  Raven's Lime is already a cool glaze, lime with tray spots and an overall metallic look.


Stars
Comment by Denice E. Demuth on March 9, 2013 at 5:39am

Kathy I haven't heard of those glazes are they premixed ones? Oh by the way the work in your new photo's are lovely as usual.  Denice

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service