Potters & Sculptors - Making Rock from Mud
Tags:
No problem there --- Ian Begg's Clear
Recipe Name: Ian Begg's Clear
Cone: 6 Color: clear
Firing: Oxidation Surface: Glossy
Amount Ingredient
50 Frit--Ferro 3134
30 Kaolin--EPK
20 Flint
100 Total
IS QUITE RUNNY BUT VISCOUS AT THE SAME TIME & WILL BEAD UP WHERE IT RUNS ONTO A KILN SHELF.
This is a berry bowl I made a long time ago...I used a ^04 glaze over a ^6 glaze ( in this case, it's glossy base 1 from Mastering ^6 with some zircopax and rutile in it) Anyway, the low fire green (and also the blue version) ran nicely on the ^6 glaze- a nice accent, but not off the pot..
The ^04 base glaze is from clayart:
Frit 3195 73
Flint 7
EPK 10
Mg Carb 10
probably 4% copper carb for green, about 2% cobalt carb for med. dark blue..
enjoy!
Tracy
Hi, Ginny. I landed here via a search for runny glazes. I would like something like this for the rims of mugs and bowls. I have a lot of portions of low fire commercial glazes. I may try a couple of these just to do something with them. Did you try the recipe that George Lewter recommended? I would like to know how they turned out.
Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase
Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com
Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.
Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.
The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.
Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .
If you are up to creating videos of your work or techniques you might want to invest in a flip video camera
Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00
And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62
ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.
If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014
Switch to the Mobile Optimized View
© 2025 Created by Andrea Wolf.
Powered by