I have been working on a yellow matte glaze. One of our interns left a bucket of glaze and it looks like the glaze on the apple baker. I have been trying to repeat the glaze and the small ikebana form is as close as I have come. I know it's an iron based yellow as the glaze is red in the bucket. The intern was heading out west and I have not been able to find her. Does anyone have any idea what I could add to mine to make it more yellow? I'm thinking some rutile. Thanks for any advice.

Jeff



Views: 3044

▶ Reply to This

Replies to This Discussion

Thanks Nancy.

Will do.... 

Looks like the yellow version of  ^6 White Bird'. 

 

neph sy         47

dolomite       10

ball clay        10

gerstly borate  23

tin oxide        5

zircopax         5

bentonite        3

Great on textured darker clay, lovely smooth matte white on white clay, not good on buff colors

 

For yellow:  add 6% rutile.  looks very much like your picture on speckled clay.  Dependable glaze, doesn't run.

 

 

It depends on your base glaze Jeff. 1-3% red iron in the right base, with a little tin (about 2%) will give a light to medium yellow. A little bit of rutile added (1-2%), may lean it toward a more warm, even peachy yellow cast.

 

In my Cone 6 Ox high alumina matt, at 8% rutile I get a deep, rich, orange. 6% give more of a deep peach, lighter as the rutile is lowered, so I would think 2% might give you a yellow in the right base.

 

 

 

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by