Hi All,

I have seen this glaze several places.  But no one willing to share.  The sample in the pic is cone 10 gas.  I'm looking for something to fire cone5/6 electric.  I will be using it over an iron heavy red clay,  Redstone by standard.

il_570xN.625122997_t1qr.jpg

Views: 1496

▶ Reply to This

Replies to This Discussion

There are several silky/satin whites that fire to cone 10. Leach white is one of them. here's a link

http://cone6pots.ning.com/forum/topics/simon-leach-glazes

Now the point is to bring this down to  cone 5/6, google is your friend, but till you make friends there,here's a  white you might like

http://www.potters.org/subject87846.htm, give it a try and see what happens

Hi Whyndham,

Thanks for the reply.  I always forget to check clayart.  Thanks.  I think I'm going to try the Pam's Frost and go from there.  I will post my results.  Will be a month or so, going on vacation.

This is my oyster glaze I use it here over white stoneware cone 6. I like how it breaks over edges. I have never used it over a dark clay but it might work.

Oyster

EPK ….......................06
Dolomite …................12
Gerstley Borate .........23
Flint …......................27
Nephelene Syenite ....32

Rutile …...............8
Chrome Oxide ..0.02

Maybe you can skip the the chrome oxide I can't remember why I added it. It is a minuscule amount but you definitely need a lot of rutile and that's dark rutile. 

Harold,

Thats one great looking glaze!  Thanks for sharing, and the heads up on the "dark rutile".  I only have light, but will be ordering some dark so I can test this glaze!

Juli

Tell me how it works out for you Juli. Try it with light rutile too.

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service