does anyone have a recipe for a base running glaze?  Yes, I know we all try hard to avoid this, but I'd like something to drip over the rim onto a colored slip surface, making nice pooly drips.  Thanks!

Views: 3339

▶ Reply to This

Replies to This Discussion

No problem there --- Ian Begg's Clear

Recipe Name:  Ian Begg's Clear

Cone:  6     Color:  clear
Firing:  Oxidation     Surface:  Glossy

Amount     Ingredient
50          Frit--Ferro 3134
30          Kaolin--EPK
20          Flint

100         Total


IS QUITE RUNNY BUT VISCOUS AT THE SAME TIME & WILL BEAD UP WHERE IT RUNS ONTO A KILN SHELF.

Very cool - and you're saying the pooling adheres to the piece rather than (gulp) to the kiln shelf?  Within reason, of course.  Have you tried adding color to this?
If your shelves have a good coating of kiln wash this glaze will sit on top rather than eating through the kiln wash and attaching to the shelf.  Picture below better illustrates this.
It ran too much for my purposes so I didn't really get into colorant testing but i'm sure it will  do alright with cobalt, copper, and iron in small amounts.
Thanks very much.  Just made up a test batch & will fire within the week.  Fun!

This is a berry bowl I made a long time ago...I used a ^04 glaze over a ^6 glaze ( in this case, it's glossy base 1 from Mastering ^6 with some zircopax and rutile in it)  Anyway, the low fire green (and also the blue version) ran nicely on the ^6 glaze- a nice accent, but not off the pot..

The ^04 base glaze is from clayart:

Frit 3195 73

Flint        7

EPK         10

Mg Carb    10

 

probably 4% copper carb for green, about 2% cobalt carb for med. dark blue..

enjoy!

Tracy

Hi, Ginny.  I landed here via a search for runny glazes.   I would like something like this for the rims of mugs and bowls.  I have a lot of portions of low fire commercial glazes.  I may try a couple of these just to do something with them.  Did you try the recipe that George Lewter recommended?  I would like to know how they turned out.

This is Reliable Albany Glaze, nice and runny. Cone 6 oxidation no hold fired with a  kiln sitter

Albany slip substitute 67

Frit 3134                     29.1

Barium Carbonate       3.9

RIO                               3

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service