Fool-(or should I say kid) proof transparent glaze........anyone have a suggestion?

My studio has begun offering classes to young, potential potters who have lots of great ideas. Unfortunately when they decorate with oxides and then want to over-glaze with a clear, the oxides run. Does anyone have a suggestion for a transparent glaze?

Views: 529

Reply to This

Replies to This Discussion

Oxides are expensive and only take a very small amt to influence the glaze color.Generally speaking, don't put oxides on bisk but in a glaze.Or have a clear or white glaze and lightly brush on an oxide was.

Most oxides will act as a flux on a glaze .

Look up clear or satin white glaze recipes on google and make test tiles with light brush strokes of oxides so folks will know what to expect before going crazy with stuff they aren't accustomed to.

Wyndham

Thank you for your recommendation! I was thinking along that line. While I do not instruct the children's courses, I will definitely set up some tiles for the classes to use.

Wyndham Dennison said:

Oxides are expensive and only take a very small amt to influence the glaze color.Generally speaking, don't put oxides on bisk but in a glaze.Or have a clear or white glaze and lightly brush on an oxide was.

Most oxides will act as a flux on a glaze .

Look up clear or satin white glaze recipes on google and make test tiles with light brush strokes of oxides so folks will know what to expect before going crazy with stuff they aren't accustomed to.

Wyndham

If you're looking for a low-fire ^06 clear, to use over the oxides or other uses, this "Idiot-Proof Clear" may interest you.

Idiot-Proof Clear ^04 - 06   -  $1.51 per pound
90.0%   Ferro Frit 3195
10.0%   Ball Clay OM4
  2.0%   Bentonite  (or use (0.2% Bentone-EW)
  2.0%   Brushing media like CMC or 1% propylene glycol

Ferro Frit 3195 melts at Cone 08. 

Adding the 10% Ball Clay helps suspend the frit and raises the melting temperature to Cone 06.

The iron contaminants in ball clay also add a yellow cast to the bluish clear of the boron frit, resulting in a more neutral-color  clear.

Although not very delicious, this glaze is at least non-toxic if eaten.

You had to have made that name up (LOL!)

With the kids doing mostly sculpture work, this may work. I have all the ingredients on hand. Thank you Norm!

Norm Stuart said:

If you're looking for a low-fire ^06 clear, to use over the oxides or other uses, this "Idiot-Proof Clear" may interest you.

Idiot-Proof Clear ^04 - 06   -  $1.51 per pound
90.0%   Ferro Frit 3195
10.0%   Ball Clay OM4
  2.0%   Bentonite  (or use (0.2% Bentone-EW)
  2.0%   Brushing media like CMC or 1% propylene glycol

Ferro Frit 3195 melts at Cone 08. 

Adding the 10% Ball Clay helps suspend the frit and raises the melting temperature to Cone 06.

The iron contaminants in ball clay also add a yellow cast to the bluish clear of the boron frit, resulting in a more neutral-color  clear.

Although not very delicious, this glaze is at least non-toxic if eaten.

A certain Lynn Goodman in New York provided the glaze name and recipe in 2006.  I've found it works well.

http://www.potters.org/subject94218.htm

http://www.lynngoodmanporcelain.com/Platters.html


Cyndy shorter said:

You had to have made that name up (LOL!)

With the kids doing mostly sculpture work, this may work. I have all the ingredients on hand. Thank you Norm!

Norm Stuart said:

If you're looking for a low-fire ^06 clear, to use over the oxides or other uses, this "Idiot-Proof Clear" may interest you.

Idiot-Proof Clear ^04 - 06   -  $1.51 per pound
90.0%   Ferro Frit 3195
10.0%   Ball Clay OM4
  2.0%   Bentonite  (or use (0.2% Bentone-EW)
  2.0%   Brushing media like CMC or 1% propylene glycol

Ferro Frit 3195 melts at Cone 08. 

Adding the 10% Ball Clay helps suspend the frit and raises the melting temperature to Cone 06.

The iron contaminants in ball clay also add a yellow cast to the bluish clear of the boron frit, resulting in a more neutral-color  clear.

Although not very delicious, this glaze is at least non-toxic if eaten.

Norm what if one is looking for a fool proof cone 6 clear with the same specs, any suggestions?


Norm Stuart said:

If you're looking for a low-fire ^06 clear, to use over the oxides or other uses, this "Idiot-Proof Clear" may interest you.

Idiot-Proof Clear ^04 - 06   -  $1.51 per pound
90.0%   Ferro Frit 3195
10.0%   Ball Clay OM4
  2.0%   Bentonite  (or use (0.2% Bentone-EW)
  2.0%   Brushing media like CMC or 1% propylene glycol

Ferro Frit 3195 melts at Cone 08. 

Adding the 10% Ball Clay helps suspend the frit and raises the melting temperature to Cone 06.

The iron contaminants in ball clay also add a yellow cast to the bluish clear of the boron frit, resulting in a more neutral-color  clear.

Although not very delicious, this glaze is at least non-toxic if eaten.

I prefer Tony Hansen's silky ^6 clear using Ferro Frit 3249 with 12% magnesium oxide or the similar frit F-69.

http://digitalfire.com/4sight/education/g1214w_cone_6_transparent_b...

I often add the additional 3% magnesium carbonate shown below.

24.8%  Kaolin
23.8%  Silica
23.2%  Ferro Frit 3134
15.2%  Wollastonite
  8.6%  Feldspar, Soda Minspar 200
  3.0%  Magnesium Carbonate

This glaze contains only 6.7% Boron Oxide contributed by the frit.  Quite a number of other cone 6 clear recipes have far more boron and so can tend to develop the bluish white borosilicate crystals known as "boron-clouding" making the glaze opaque in areas, or worse can develop crazing.

A quick and easy solution can be a combination of Ferro Frit 3134 with kaolin, at a ratio of say 70% / 30% depending on how fluid you want the clear  to peak temperature.

Nadine Mercader said:

Norm what if one is looking for a fool proof cone 6 clear with the same specs, any suggestions?


Norm Stuart said:

If you're looking for a low-fire ^06 clear, to use over the oxides or other uses, this "Idiot-Proof Clear" may interest you.

Idiot-Proof Clear ^04 - 06   -  $1.51 per pound
90.0%   Ferro Frit 3195
10.0%   Ball Clay OM4
  2.0%   Bentonite  (or use (0.2% Bentone-EW)
  2.0%   Brushing media like CMC or 1% propylene glycol

Ferro Frit 3195 melts at Cone 08. 

Adding the 10% Ball Clay helps suspend the frit and raises the melting temperature to Cone 06.

The iron contaminants in ball clay also add a yellow cast to the bluish clear of the boron frit, resulting in a more neutral-color  clear.

Although not very delicious, this glaze is at least non-toxic if eaten.

That opaque or bluing is what I want to avoid. I will try as you directed with he addition of magnesium carbonate. Thanks for the help.

Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014