• Does anyone know the recipe for the Bailey's Red that Stephen Hill mentions in the video and uses. He does not include this recipe with the DVD (probably because it is published by Bailey somewhere else?)...

Views: 3209

▶ Reply to This

Replies to This Discussion

Hello Tom:

I too was looking for the Bailey's Red recipe.  I realize that I owned the "Glazes Cone 6" book by Michael Bailey and that recipe might be in the book.  In the book he has a chapter dedicated to a Red/Orange glaze.  I suspect this is the Bailey's Red that Steven Hill is referring to.  Below is the recipe.

One interesting note about the Steven Hill glaze list that came with his DVD.  I was talking with a potter who had the good luck of taking Steven Hill's week long class at the John Campbell Folk school.  He told me that Steven mentioned to the class that there was a typo in one of the recipes.  In the "Hanna's Fake Ash" recipe, the percentage for the colorant Bentonite is suppose to be 1.1%  Not 10%.  Good luck.

Graham

Here is the Bailey's Red recipe:

Potash Feldspar 46.7

China Clay 4

Bentonite 2

Bone Ash 15

Lithium Carbonate 4

Talc 16.9

Flint  or quartz 11.4

Color

Red Iron Oxide 11.5

Hello Graham,

I just saw your note about Hanna's Fake Ash from Steven Hills DVD, and when making up a card with the correction I realized that the materials recipe itself actually doesn't add up to 100% (it totals 122.7). Do you have the correct numbers?

Arthur 

Do you have any information about food safety with Stephen Hill's Glazes? Specifically, Strontium Crystal Magic, (Cool and Warm versions), SH Watercolor Blue and Green? I notice he uses these on the outside of mugs up to the edge of the drinking vessels, which obviously implies oral contact with these glazed surfaces. 

I have used a Bailey Red for a long time. I don't even remember where I found it. 

ball clay 13

silica 14

potash feldspar 44

talc 10

magnesium carbonate 3

bone ash 14

RIO 11

Hi Marina, is the Baileys Red your referring to also a cone 6?

And is there a particular way of applying the glaze eg. thin to get the speckles or is it the firing schedule? thank you 

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service