From John Britt

Magruder Red cone 6

Here is a really nice cone 6 Iron red. Don't have an image but trust me- it is nice!

If you get an image - send it to me and I will post it.

Magruder’s (Iron ) Red cone 6 oxidation
44.8 Kona F-4
12.3 Silica
18.2 Talc
16.1 Bone Ash
  4.3 EPK
  4.3 Lithium Carbonate

2. Bentonite
12.3 Synthetic Iron Oxide
I would like to try it out. Anyone already worked with this?

Views: 952

Comment

You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!

Join Electric Mid&Hi Fired Ceramics

Comment by Rathissh Ceramics on April 26, 2012 at 2:42am

Rathissh Ceramics, Virddhachalam, Tamil Nadu, India is one of the leading Manufacturers, Suppliers and Exporters of Ceramic Products, Ceramic Toys, Plaster of Paris Powder, Refractory, Procelin Special Items, Vegetables and Herbal Products.
Ceramic Toys

Comment by Sylvia Shirley on February 21, 2012 at 12:48pm

Joan,

Thanks for all the information!  I love that article on iron oxide and can't wait to experiment with the glaze they have listed there.  

I haven't had a lot of time to explore this web site yet.  There seems to be a ton of good information.  I could get lost in here.  I will try to put up some photos of my work that are more appropriate than this thumbnail.  It's actually a cone 10 gas glaze.  I'll switch to one that's cone 6.

Sylvia


Stars
Comment by Joan Scott on February 21, 2012 at 12:34pm

Hi Sylvia,

I had never heard of synthetic iron before either. It is described here in a pdf by John Britt http://ceramicartsdaily.org/wp-content/uploads/2011/03/cmtechnofile...  Very interesting article and another description here http://www.potters.org/subject83623.htm/  and I am sure you can find other articles about iron. It really is interesting. And you must have read this article http://ceramicartsdaily.org/ceramic-glaze-recipes/glaze-chemistry-c...

You don't have any examples of your work. The one that is your photo is interesting but very small. How about uploading some pieces?

Joan

Comment by Sylvia Shirley on February 21, 2012 at 7:58am

Where do you get Synthetic Iron Oxide?  I've never heard of it.

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service