Check this out- same glaze, different cooling cycle- Red from MC6 Waterfall Brown

I have been trying to get iron red out of my kiln ever since I replaced it. Kept trying to slow cool from 1800 F down to 1500 F- This is proving to me that the "sweet spot" is lower in temp than I've been going. In an attempt to save a load of tableware through its slow cool cycle after my sitter tripped and stopped the kiln, I ramped it back up from 1227 up to 1800 and then slow cooled, 150 per hour to 1500. Somewhere in the process I turned all of my brown dishes red/orange. After putting them back in the kiln and refiring to cone 6, they darkened up to a much nicer red, with dark flecks and fun stuff on the surface. They don't match the rest of the set, but they are kind of cool.

The saga continues.

8/18 update(and note to self): 1250 degrees is not hot enough. I did a low bisque of pots (^018 with a 15 min hold) with terra sig on them for a barrel firing and threw in some wfl brown test pots to see if they'd turn. No dice. Next test will be closer to 1500, I guess.

Latest- magic temp for me is 1650 F with an hour hold- I then slow cool, 150 per hr, to 1400.

Views: 1537

Comment

You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!

Join Electric Mid&Hi Fired Ceramics

Comment by Tracy Shea on May 2, 2010 at 7:40pm
No, just down from 2174 to 1227F. then, I ramped back up to 1800 and cooled @ 150 per hour to 1500.
Comment by Kitoi on May 2, 2010 at 6:13am
Great results!

So the kiln cooled completely then you ramped it back up and slow cooled?

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2025   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service