Comment by Norm Stuart on March 22, 2014 at 9:32pm

The red or pink of chrome-tin glazes is easily decomposed into a non-colored glaze by other glaze chemistry.

So in a battle of chrome-tin raspberry poured over some other glaze, very little of the raspberry color remains intact.  I suspect even less red or pink would be visible if the other glaze were applied over the chrome-tin.

Comment by Jennifer Arthur on March 22, 2014 at 7:13pm

Raspberry over Warm jade.

Comment by Lawrence Weathers on March 18, 2014 at 4:20pm

is this raspberry over green jade or the other way around?

Comment by Jennifer Arthur on March 4, 2014 at 3:27am

Recipe Name: Warm Jade
Cone: 6 Color: GREEN
Firing: Oxidation Surface: Glossy
Amount                 Ingredient
44                           Nepheline Syenite
25                           Gerstley Borate--1999
19                           Silica
12                           Ball Clay Number 1
100                         Total

 Additives
3              Copper Carbonate
4              Rutile
5              Tin Oxide

Comments: Adjusted from Chappell's Floating Blue. Gives a nice warm jade green glaze. Three thick coats brushed.

Great green glaze. 4% copper carbonate will give an iridescent green. 2% copper carbonate will give a celedon light green.

70 - Raspberry C/6     

 

Whiting                                  20%

Neph Syenite                          18%

Frit 3134                                 14%

Om-4 Ball Clay                      18%

Silica                                       30%

Green Chrome Ox                .02%

Tin Oxide                               7.5%

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service