Potters & Sculptors - Making Rock from Mud
Rovin White Porcelain
cone 6 oxidation
••••••
Recipe Name: Penland Red-Orange
Cone: 6 Color: red
Firing: Surface:
Amount Ingredient
46.7 Feldspar--Kona F4
16.9 Talc
15 Bone Ash
11.4 Flint
4 Kaolin--EPK
4 Lithium Carbonate
2 Bentonite
100 Total
Additives
11.5 Crocus Martis
Unity Oxide
.118 Li2O
.12 Na2O
.054 K2O
.289 MgO
.418 CaO
1.000 Total
.242 Al2O3
.002 Fe2O3
1.989 SiO2
0 TiO2
.099 P2O5
8.2 Ratio
6.8 Exp
Comments: replace kona f4 feldspar with minspar
-----------------------------------
Calculations by GlazeMaster™
www.masteringglazes.com
------------------------------------
                                            Tags:
                    Albums: Finished Bowls and Mugs                        
                                        
                
Comment
Hi Norm,
So how pure is the "Special Red Iron Oxide" from Ceramic Supply? It is the one that I have been using lately for my RIO. Also I have been using the purple stuff for Crocus Martis, but like I said before, I also have used another purple hematite that I got from an art supply place that mainly caters to oil painters, so this was a pigment that is used in oil painting. Just wondering. jeff
Here's the iron oxide sourcing information from U.S. Pigment.  http://www.uspigment.com/chemicals.shtml
Our High Purity Iron Oxide is from China and is about 99.5% average.
Spanish Iron oxide is the same what every one is selling, its about 82% iron oxide and it is imported by Hammill and Gillespie and is distributed all over the country.  (I assume this is Promindsa's Prominfer product)
Pink Iron Oxide is also from China and is about 80% iron oxide.
Natural iron oxide is mined in Michigan and is only 70% iron oxide.
Yellow Fe3O4 is a food grade C.I. Pigment Yellow 42 made by Bayer.
(Most iron oxides from China are copies of one of the Lanxess Bayferrox pigment products, licensing their production techniques from Bayer - at least as soon as Bayer finds them and sues them)
Norm, I could do some research. Whatever this is certainly acts differently than any other iron oxides I've used.
Where do you buy your Crocus Martis, or do you know what it consists of?
Each ceramic supplier provides commercial iron pigments for each type of iron oxide or crocus martis they supply, but it seems few suppliers choose the same commercial iron pigment for each type of iron oxide.
When asked for "Crocus Martis", which has not been available for many years, some suppliers say it's not available, some sell "Spanish Iron Oxide" as crocus martis, which is usually a product called "Promifer", mined by Promindsa in Spain, but some suppliers provide one of the six Promindsa "Micronox R" products instead as "Spanish Iron Oxide". http://www.promindsa.com/product/
Other suppliers sell a mind-boggling array of synthetic commercial iron pigments as Crocus Martis.
Here's Digitalfire's general take on it. http://digitalfire.com/4sight/material/crocus_martis_249.html
The Crocus Martis supplied by Standard Ceramic is Bayferrox 130, which is 96% Fe2O3 and 3% Silica and Alumina. While their red iron oxide precipitate is Bayferrox 140 which is only 94.2% Fe2O3.
Highwater supplies Bayferrox 180M when asked for Crocus Martis, and a partially natural product called RedCAST® from Prince Minerals as Red Iron Oxide. http://www.highwaterclays.com/index.cfm?fuseaction=feature.display&...
http://www.highwaterclays.com/index.cfm?fuseaction=feature.display&...
The Crocus Martis New Mexico Clay sells is also Bayferrox180 which they describe as "Purple Iron". http://www.nmclay.com/Amazing/itemdesc.asp?ic=CROCUSMARTIS
They sell Yellow 569 as yellow iron oxide, which is 98% FeO-OH and 2% silica.
http://bayferrox.com/en/products-applications-bfx/product-search/ba...
The look of your glaze is similar to Orange Street glaze I make with Bayferrox 503, or preferably Bayferrox 222, in place of red iron oxide. http://bayferrox.com/fileadmin/pdf/IPG/56190590_000_BF-503-ENG.pdf
http://bayferrox.com/fileadmin/pdf/IPG/00006319_000_BF-222-FM-ENG.pdf
When a recipe like Orange Street calls for both red iron oxide and crocus martis, I use yellow iron oxide from Laguna Clay/Axner in place of the crocus martis, which seems to create the right glaze color.
Although Laguna Clay describes their "Yellow Iron Oxide" as "A weaker form of iron—high clay content",
the MSDS for their Yellow Iron Oxide actually lists >99% pure CAS-51274-00-1 aka (FeO-OH) - hey, where's this alleged "high clay content"? http://www.axner.com/ironoxide-yellow.aspx
It leaves us ceramacists without much actual guidance when a recipe calls for red iron oxide, yellow iron oxide, or crocus martis. They're names without much specific meaning.
Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase
Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com
Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.
Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.
The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.
Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .
If you are up to creating videos of your work or techniques you might want to invest in a flip video camera
Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00
And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62
ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.
If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014
    © 2025               Created by Andrea Wolf.             
    Powered by
    
    
You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!
Join Electric Mid&Hi Fired Ceramics