Slip drizzled and brushed on. Glazed with clear glaze.

Views: 107

Comment

You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!

Join Electric Mid&Hi Fired Ceramics

Comment by Jan Wallace on October 28, 2011 at 4:06pm
Thanks George. That is brilliant. I will test some in my next glaze firing and let you know how i go. :)
Comment by George Lewter on October 28, 2011 at 10:53am

Recipe Name:  5-6 Clear
Cone:  6     Color:  clearFiring:  Oxidation     Surface:  Glossy
Amount Ingredient

40          Feldspar--Kona F4

30          Gerstley Borate--1999

20          Ball Clay--Old Mine #4

10          Silica

100         Total

Unity          Oxide

.3           Na2O

.113           K2O

.01           MgO

.576           CaO

1.000          Total
.768           Al2O3

.558           B2O3

.008           Fe2O3
4.541           SiO2

.015           TiO2
5.9          Ratio

6.9            Exp
Comments:  From U Florida midrange glaze base. "Boy, do I have a fabulous clear glaze for you!! I tested about 15 clears last year and only came up with 2 that I would consider using. This glaze is incredibly forgiving - doesn't show drips, overdips, differences in thickness, is glassy clear w/o yellow, and doesn't craze. Can you believe it? I couldn't either, but it's true and I am absolutely thrilled with this glaze. It only has 4 ingredients, too. I use this over slips and underglazes and it's fine. I also use lusters over it with great results. What can I say? This is THE PERFECT clear glaze. Have fun. Laura in Oregon"  -----------------------------------Calculations by GlazeMaster™

Comment by Jan Wallace on October 28, 2011 at 1:53am
Hi George, is the clear glaze you have used here posted on this site by any chance. I have tried a few clear Cone 6 glazes lately, with no real satisfaction. Can you help please? Thanks in advance.

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2024   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service