The look of 10% nickel carbonate in a high expansion Ferro Frit 5301. Using Ferro Frit 3269 the green crystallization is less widespread, typically where the glaze pools.
I'm adding EPK and other ingredients to replicate this glaze for ^6.
Tags:
Comment
Off the top of my head I added 10% EPK, which doesn't seem at all sensible now.
Upon reflection it seems I should add only 20% to 25% Silica to make it more refractory, with a Silica/Alumina ratio similar to other glossy high fire glazes.
What I meant was how much of what are you adding to the recipe before you take it up to ^6? I could try some variations as well to see what we can come up with. Jeff
I'm trying a ^6 without slow-cool tomorrow.
There are samples of the 100% 5301 and 20% Iron Oxide, with pancakes underneath, as well as the same with added Kaolin or Kaolin and Silica. I don't know enough not to try it.
The tile below is fired to ^06. The Glaze is 100% Ferro Frit 3269, 20% Spanish Iron Oxide, with 16% Cryolite added to bring the Fluorine up to the 9% level found in the 5301 frit. With the Cryolite added I get Aventurine.
Clearly Fluorine is an important ingredient for a nice Aventurine glaze, likely as a flux but who knows what else it contributes? I previously tried recipes without Fluorine, like the ones below the photo, which result in a more opaque Aventurine glaze which splatters in the kiln which is not anyone's idea of a good glaze.
Ugly Muddy Kiln Splatter Aventurines (too thick and they're matte brown)
http://lindaarbuckle.com/handouts/glz_hg_lowfire.txt | |
124.0% | Aventurine ^04 |
75.0% | Gerstley Borate |
25.0% | Silica, Imsil A-25 |
24.0% | Red Iron Oxide |
105.6% | Aventurine ^04 John W Conrad |
39.7% | Silica |
38.8% | Borax |
15.2% | Red Iron Oxide |
7.0% | China Clay |
2.7% | Boric Acid |
2.2% | Barium Carbonate |
How hard is that going to be to take it up to ^6? Would you be able to do that with the Iron Aventurine as well?
Hey Norm,
That's a cool looking glaze! 5301 does some nice things. I still haven't gotten around to making the aventurine with the Special RIO. Maybe this weekend!
Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase
Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com
Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.
Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.
The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.
Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .
If you are up to creating videos of your work or techniques you might want to invest in a flip video camera
Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00
And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62
ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.
If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014
Switch to the Mobile Optimized View
© 2025 Created by Andrea Wolf.
Powered by
You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!
Join Electric Mid&Hi Fired Ceramics