Recipe Name:  Lemon Frost Matte

Cone:  6     Color:  Pale Yellow

Firing:  Oxidation     Surface:  Matte

Amount     Ingredient

60          Nepheline Syenite

20          Strontium Carbonate

1          Lithium Carbonate

10          Ball Clay--Old Mine #4

9          Silica

100         Total

               Additives

5          Titanium Dioxide

10          Cerdec Degussa Yellow Stain

2            Bentonite

The base of this glaze was developed by Pete Pinnell, (Pinnell's Strontium Matte).

Calculations by GlazeMaster™

www.masteringglazes.com

------------------------------------

Comment by Jan Wallace on June 21, 2012 at 12:07am

Joe that is a beautiful glaze. Yellow is a difficult colour to achieve successfully. Is it Cone 6 and if so would you care to share the recipe please?

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2025   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service