Comment by Paul Boland on June 6, 2014 at 9:03am

it is sometimes fickle. prone to pinhole if to thick.

Comment by Cyndy Littleton on June 6, 2014 at 9:00am

Gorgeous and easy. I like it!


Stars
Comment by Paul Boland on June 6, 2014 at 8:58am
honey w/iron 6 ox
ingredients %   5000g lb 10,000g
dolomite 20.00%   1000 2.20 2000
frit 3134 20.00%   1000 2.20 2000
spodumene 20.00%   1000 2.20 2000
ball clay 20.00%   1000 2.20 2000
silica 20.00%   1000 2.20 2000
      0 0.00 0
bentonite 2.00%   100 0.22 200
manganese dioxide 3.00%   150 0.33 300
RIO 5.00%   250 0.55 500
* dark clear no “bluing” effects     0 0.00 0
Comment by Cyndy Littleton on June 6, 2014 at 8:43am

Do you mind sharing the recipe for the honey amber?


Stars
Comment by Paul Boland on May 17, 2014 at 4:15pm

^6 ox Metalic Black cups

Bowls: Matte White over Tenmoku, Honey amber over black engobe (2)

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service