Comment by Maulik Oza on May 21, 2013 at 9:15am

hi,

recipes for glazes which you have asked for..

For Green, molten  grey green and clear coat with slip decoration.

Base glaze (transparent gloss):

gerstly borate frit  26

soda feldspar        48

china clay             6

silica                    20

For green  add chrome oxide 5%

for grey green add Red iron oxide 2%

                            Rutile             5%

recipe for first white glaze near to green one (satin finish):

gerstly borate frit  21

soda feldspar         16

china clay              11

whiting                  20

silica                      32

recipe for another white glaze ( which again didnt come out properly):

gerstly borate frit   50

china clay               15

silica                      35

i hope i have answered all your questions. if anything else i will be happy to answer.:)

Comment by Maulik Oza on May 20, 2013 at 8:38pm

Hi brian,

i will try to answer all your questions one by one.

those textured metallic tiles are not silicon carbide glaze. it is not properly melted or over fired i dont know, so it is in bubbling stage. if you know anything about it like why this thing happens let me know.

those two white ones are with zinc oxide i will write you the recipes by evening.

green one is with chrome 5% in base glaze. ( recipe i will post it in the evening )

rutile is the magical secret ingredient for all my molten glazes. whenever i find any glaze little dull i add 5% rutile in it and it becomes live :) ( i have just entered in ceramic world so till now whatever i have done in that it has worked for me :P )

brown with lines is just clear base glaze coat on slip decoration. ( slip is made up of ball clay and  5% red iron oxide ) i generally use this slip for writing down the recipe number at the bottom of the test tile. no no it is not carved it is just pained with brush first and then dipped in to clear glaze.

thank you for your questions and showing interest in my work i will get back to you with recipes in the evening..

-oza

Comment by Maulik Oza on May 20, 2013 at 1:15am

Thanks norm..:)


Stars
Comment by Norm Stuart on May 19, 2013 at 11:14pm

An interesting way to make test tiles.

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service