i noticed that the ratio of strontium to lithium in the steven hill glaze was 4:1. I thought it might be interesting to see what that would do sprayed on my glazes, before adding new glazes to my studio. Both mugs are glazed the same. The one on the right has the stron/lit spray (20g stron, 5 lith, 100 H20)...I may have sprayed too much (i'm not a sprayer) ....it definately added flow, maybe a little crystalization? the second pix is a little out of focus. these fired to cone 6 and were on the same shelf, next to each other
Tags:
Comment
thanks, I've been working with this base for almost 16 yrs, and every time I think I'm done with it, I get excited about it again--I'm looking forward to seeing what your results
Thanks again Donna. I understand now that you sprayed the stront and lithium over the white and green glaze. This certainly is a lovely glaze with some great variations when colourants are added, but you have a flair for decorating and your technique obviously makes for your great results. I will let you know how I go. :)
hi Jan
no , I just sprayed a mix of stron/lith as stated above. the glaze had the cu. here is the recipe. this glaze was given to me by Andy Quient. I have not tested it for food safety, though it has been in my dishwasher hundreds of time, and i never store food in my ceramic ware, I suggest if you use it, you test it.
Andy Quient's copper matte (in percentages)
Corn stone 21%
Ferro 3134 22
Dolomite 21
om4 ball clay 15
flint 20
__________________
99
Bentonite 2%
CuCo3 4%
water 9 qts 19 oz including cleaning bucket out
it is a great base, I have tweaked it over the years with great results....
the white glaze (which is allover coverage) is this base glaze w/o colorants matte white...its not too noticeable, but the spray also shined up the white
the base plus 1/2 % cobalt oxide is a matte periwinkle blue
Donna, Did you add any copper or colourant to the spray mixture? Or, is this green totally a result of the stront, lithium and water mix that you sprayed on? Also, what glaze did you spray over as this obviously plays a part in the end result? Thanks. Jan
Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase
Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com
Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.
Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.
The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.
Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .
If you are up to creating videos of your work or techniques you might want to invest in a flip video camera
Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00
And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62
ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.
If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014
© 2025 Created by Andrea Wolf.
Powered by
You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!
Join Electric Mid&Hi Fired Ceramics