Recipe Name: 72 Base with Rutile

Cone: 6 Color: white
Firing: Oxidation Surface: Semiglossy

Amount Ingredient
24 Nepheline Syenite
11 Dolomite
12 Gerstley Borate-Laguna
4 Whiting
2 Zinc Oxide
7 Kaolin--EPK
40 Flint

100 Total

Additives
8 Rutile

Unity Oxide
.144 Na2O
.04 K2O
.214 MgO
.525 CaO
.077 ZnO
1.000 Total

.259 Al2O3
.145 B2O3
.003 Fe2O3

2.998 SiO2
.001 TiO2
0 P2O5

11.6 Ratio
6.6 Exp

Comments:
-----------------------------------
Calculations by GlazeMaster™
www.masteringglazes.com
------------------------------------

Views: 301

Comment

You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!

Join Electric Mid&Hi Fired Ceramics

Comment by Shine Chisholm on March 3, 2014 at 8:44am

This base is very nice with mason stains-- I posted a couple of picture using yellow, purple, and orange. I'm planning a batch with cobalt carbonate soon.

Comment by George Lewter on March 2, 2014 at 9:30am
Interpreting the Base 72 Rutile recipe.
The base is the first set of ingredients adding up to 100. Mix those ingredients to make a very small test batch or multiply them each by a factor of 5, 10, 20 or whatever to get a batch of the size you want. (500g, 1000, 2000, etc.) Whatever the total, You then add 8% of that total of rutile to the batch.
The unity oxides are just the chemical breakdown of the ingredients you have in that recipe and are useful for studying the characteristics of the glaze.

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service