Potters & Sculptors - Making Rock from Mud
Rather than reinvent the wheel when it comes to the large topic of ceramic colorants I am going to refer to the ceramics department manual from San Francisco State University that is generously posted with public access.
http://www.sfsu.edu/~ceramic/classmanual.htm - the whole manual
http://www.sfsu.edu/~ceramic/manual/colorants.htm - the colorants section
It appears that the online materials were possibly scanned from paper documents and then run through OCR software to produce the digital content. I noted numerous formatting inconsistencies and a number of cases where quantities were not given.
The following is extracted from http://seco.glendale.edu/ceramics/glazebasics.html, and is a very compact listing of common colorants and percentage ranges.
CHROME OXIDE - Usually added to glazes to produce greens in reduction firings. However, combined with tin, pinks can be produced. If zinc is present in the glaze, a brown will result. Browns are also produced in oxidation firings. Use in 2-3% amounts.
COBALT OXIDE or CARBONATE - Both are common cobalt sources and invariably yield blues in glazes, both reduction and oxidation. If magnesium is present in the base glaze, blue violet colors will result. Use in 1/2% to 2% amounts.
COPPER OXIDE or CARBONATE - Copper yields blue and green colors in oxidation glazes, and red to purple colors in reduction glazes. However, any barium present in the base glaze will cause copper to yield blues even in a reduction glaze. Use in 2-5% amounts.
IRON OXIDE - The most common glaze colorant, used to color clays, slips, washes and glazes. In high temperature, reduction glazes, it tends to develop into celadon colors in concentrations below 2%. In higher amounts, yellows, oranges, golds, brick, brown and black colors can result in reduction firings. Iron is a powerful flux also, so beware glazes running if you increase the iron concentration towards 8%.
MANGANESE DIOXIDE or CARBONATE - A relatively weak colorant which produces browns in reduction firing, and purples in oxidation firings.
NICKEL OXIDE or CARBONATE - A versatile colorant, producing many colors from blue to tan to gray to green depending on base glaze composition. Most often used to soften the effect of another colorant. Used frequently in crystalline glazes. Use in 1-3% amounts.
RUTILE - An impure oxide of titanium which contains iron oxide as well. Used alone, it produces tans and tends to make a glaze more opaque (see below). Most often used in combination with iron oxide and other oxides as a texturizer. Use in 3-5% amounts.
VANADIUM PENTOXIDE - A weak yellow colorant, often combined with tin oxide for stronger yellow. Used in oxidation only, as it produces dull grays in reduction firing. Use in 5-10% amounts.
A somewhat better presentation and layout is a pdf handout from Linda Arbuckle at:
(Linda Arbuckle's website has a whole list of handouts and articles stemming from her years as a prominent ceramics educator)
None of the forgoing delve into stains and encapsulated stains which can be used to very good effect where strong solid color is desired.
Anyone who finds better information on the use of colorants is encouraged to post it as commentary to this discussion.
Related content at:
Tags:
My brightest Pink is produced by a glaze with Tin, but has not even trace amounts of elements which are reported to create pink when combined with tin, such as chrome or manganese. The glaze does have a very high concentration of Boron, from the 3134 Frit which could be reacting with the tin to make pink? Typically high Boron levels are reported to inhibit pink colors.
Digitalfire Color Listing: http://digitalfire.com/4sight/properties/ceramic_property_glaze_col...
Powderbox Pink - the mystery is where the pink comes from
| 50.0% | Ferro Frit 3134 |
| 25.0% | Silica |
| 15.0% | Ball Clay OM4 |
| 7.0% | Tin Oxide |
| 5.0% | Calcium Carbonate (Whiting) |
Nice pink. If you don't mind I shall try it and see what happens. I'll let you know.
Many years ago I glazed a large pot with a white matte glaze in wide alternating stripes with a chrome green. It was reduction fired to cone 10. I believe some of the chrome fumed off and was absorbed onto the white, turning it to a beautiful pastel pink. Fume effects have been widely reported over the years with many effects possible.
This plate was the "Mastering Cone 6 Glazes" ^6 Majolica, but made with 10% Tin Dioxide rather than less expensive 16% Zircopax.
A vase glazed with a chrome glaze was fired on a half-shelf just above this piece, so I got a uniform pink rather than a white.
This piece is old enough that it's been through the dishwasher a few times after it collects dust.
| 116.00% | Majolica ^6 |
| 23.00% | Nepheline Syenite |
| 23.00% | Ferro Frit 3124 |
| 23.00% | Silica |
| 17.00% | Kaolin - EPK |
| 14.00% | Whiting - Calcium Carbonate |
| 10.00% | Tin Dioxide |
Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase
Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com
Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.
Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.
The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.
Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .
If you are up to creating videos of your work or techniques you might want to invest in a flip video camera
Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00
And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62
ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.
If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014