Recipe Name: Val's Turquoise Matte Cone: 6 Color: turquoise Firing: Oxidation Surface: Dry Matte Amount Ingredient 60 Nepheline Syenite 25 Strontium Carbonate 9 Flint 4 Kaolin--EPK 2 Lithium Carbonate 100 Total Additives 3.5 Copper Carbonate 4 Bentonite 1 Epsom Salts Unity Oxide .08 Li2O .284 Na2O .088 K2O .005 MgO .037 CaO .507 SrO 1.000 Total .454 Al2O3 .001 Fe2O3 2.325 SiO2 0 TiO2 0 P2O5 5.1 Ratio 9.2 Exp Comments: ----------------------------------- Calculations by GlazeMasterâ„¢ www.masteringglazes.com ------------------------------------