Hello All, 

I am just venturing into Once Firing and my pieces are stoneware with underglaze and I'd welcome any advice/insight about covering the underglaze with Cone 6 (zinc free) clear.

Any problems with once firing this combo?
Any adjustments to firing schedule recommended?

Thanks!

KarenB

Views: 407

Replies to This Discussion

Underglaze should not present any problems. The following might be a good clear for you to try with your UG and clay body.

Recipe Name:  5-6 Clear
Cone:  6     Color:  clearFiring:  Oxidation     Surface:  Glossy
Amount Ingredient

40          Feldspar--Kona F4

30          Gerstley Borate--1999

20          Ball Clay--Old Mine #4

10          Silica

100         Total

This glaze has enough clay to allow it some shrinkage with the body clay.

Kona F4 spar is soon to be extinct, so you might try to buy a full bag if you can get it at all. T

Thanks for your reply George and for the much appreciated recipe and 'heads up' about Kona F4!
K

Hi....I have tried once firing with satin glazes over my sculptures and vases...because I don't want a glossy finish...I usually get some clouding of the clear satin glaze...which can be a nice effect...but if I want it truly clear and matte to satin...I do my bisque fire all the way up to cone 6 with the underglazes ....and tweek the underglazes again sometimes at a low fire and  and then do a low fire 05/06 satin matte glaze...I should say most of my work is sculptural ...

 

 

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service