Gas kilns use hard fire-brick which cool far more slowly than the foam-core brick used in electric kilns. Many here have suggested this is one major difference in the "cone 10" look of a gas kiln.

Using our Cress E23 computerized kiln controller we slow the rate of cooling between 1,800F and 1,500F.

Over the past two years I have used three different cooling rates: 185F per hour, as suggested in "Mastering Cone 6 Glazes"; 100F per hour; and 50F per hour. We finally settled on 50F as the rate we preferred.

Some glazes become so crystallized and matte at 50F cooling I need to add 10% Ferro Frit 3268, or slightly more, to give them enough flux and silica to retain their look.

These are photos of Ron Roy's Sapphire cooled at 185F, 100F, and 50F.

Views: 7817

Reply to This

Replies to This Discussion

Kathryn - All of the recipes for the glazes I use are available on George Lewter's Insight Live Users Group. Send George an email to join at this link, and he'll send you a log-in ID.

http://cone6pots.ning.com/group/insight-live-users-group

This is the website of Jayne Shatz, whose glaze this is.  -  http://www.jayneshatzpottery.com/

And this is the recipe in Insight Live


Kathryn Reedy said:

Hi,Norm,

I've searched to the end of the internet for this recipe (Shatz Blue Matte)with no luck! Can you share the recipe?

Thanks!


Norm Stuart said:

Another typical difference between slow-cooling at 185 F/hr and 50 F/hr with Jayne Schatz Blue Matte.


 

Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service