Simon Leach Pottery video - entitled Pitcher double dip + PB glaze recipe

https://www.youtube.com/watch?v=GQgp9FtYoFE&list=PLDDEBe7QOmgGe...

Simon uses an off white glaze as a base  "PB", which he then paints with a blue wash, and "an iron oxide."

the PB off white glaze is discussed in the video, and is a cone 10 reduction

any chance we can modify in oxidation, cone 6 ? (white stoneware)

this is similar to light greyish base pots with cobalt and/or iron oxides applied, which is the general effect i am looking for 

recipe listed on the video, and for completeness is listed as follows:

PB glaze - from Bernard Leach’s recipe , he doesn't  know what PB stands for

Off white base glaze

Flint 4 lbs

Kaolin 2 lbs 12 oz

Feldspar 3 lbs 14 oz

Whiting 1 lb 14 oz

Talc 1 lb 2 oz

Blue wash:   no amounts listed. :(

cobalt

red iron oxide

manganese dioxide

iron oxide - no idea what recipe :(

thanx for help,

cp - on the pond, which is overflowing due to beavers blocking the outflow.

 

Views: 2401

▶ Reply to This

Replies to This Discussion

The old standby trick to reduce the maturing temp of a cone 9-10 glaze is to replace 50-100% of the feldspar with nepheline syenite. This is guaranteed to work perfectly - Not!

The dipping technique, from the video, where you don't have to wax the feet is terrific.

Adding red iron oxide, however, that might give you gray-green in reduction, is likely to remain brown in oxidation (the celadon variation Simon was talking about). You might need to go to a different colorant or stain.

thank you kindly 

reply by Simon Leach about Blue Wash recipe on his video:

Hi CP

The blue wash is 
25% of each of these :
Cobalt oxide
iron oxide
manganese dioxide
dry crushed porcelain clay
Sieve all ingredients - 100 mesh
Use as a decorating pigment or watered down as a wash. Experiment with application thickness.
Best Simon

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service