Hi,

I've been trying to work out a raw glaze recipe, after reading a few books suggesting ball clay works better for raw glazing leather hard pots. This glaze is intended to fire to ^8 and will be in an electric kiln, although perhaps gas firing in the future. I'm planning to make up a kg or so to test. Just wondering if anything sticks out as problematic to anyone? It is withing the green and copper limits for this cone range, and expansion seems ok according to a glaze simulator I used. 

Thanks! 

Tom

BallClay2
HP 71 Ball Clay 32.00
BPS Soda Feldspar 32.00
Quartz 14.00
Wollastonite 12.00
BPS Calcium Borate Frit 10.00

Views: 967

▶ Reply to This

Replies to This Discussion

I have some bentonite I could add if needed after a bit of testing

Tom:

HP71 has 0.80% iron with 19% alumina. Old Hickory #5 has 0.88% iron! but nearly 30% alumina. Just as alumina gives glaze strength, it likewise does the same for clay. In short, #5 will make your glaze stronger and more resistant to cutlery marks. At cone 8, the 32% soda spar is probably right on the border for a melt; most cone 6 recipes typically have 50%. 

Tom

By the way, with that much ball clay, bentonite for suspension should not be required.

Thanks Tom, my local UK supplier only sells hp71 ball clay so I'm stuck with that for now. I guess I could reduce the quartz if alumina is too low? But I suppose that will result in Matt glaze. When your say right on border you mean only just melting and ^8 ? 

Tom:

Look at the glaze this way: a standard porcelain clay body is 50% kaolin, 25% silica! and 25% feldspar. Your glaze recipe has 32% clay content; the most I have seen prior to is 20%.  If cone 6 glazes average 50% spar, I would guesstimate 40% minimum at cone 8. With that amount of clay content, it will need some added flux to melt it. 32% clay content will require more flux and heat! and will tolerate more flux and heat.

i looked up some info on Potclay's site in the UK. hVA/R 3408 has 27% alumina, 0.90% iron! and zero carbon content. You have pay closer attention to carbon content when using clay in a glaze. Carbon plays a role in pin- holing and bloating: so 0% carbon is well suited for a glaze recipe.

Tom

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service