I continue to have problems with surface bubbling. Sometimes it is a very fine bubbling just under the surface. I am stumped - sometime it happens and sometimes it doesn't. I am using a Grolleg cone 4-6 clay from Clay art. The main glaze is the cone 6 majolica from Mastering cone 6 glazes, I also use their firing schedule. I have been having this ongoing dilemma for over a year. The pieces are medium to large covered jars with smooth surfaces.  I would love any mentoring concerning working with porcelain. I have been working with clay for many years and this is how I make my living.

Views: 321

Reply to This

Replies to This Discussion

Pamela
I also left you a message on your page, but here is some further information on your problem that might help. http://www.lagunaclay.com/support/bloating-and-blackcoring.php

The prior studio facilitator bought some cone 4 porcelain which bloated at cone 6, even after a hard bisque with a 20 minute hold.  Something in the clay decomposed in the heat at cone 6. The more you fired those pieces the more they would puff-up and warp like a Pillsbury dough boy.

The piece below was covered with a Cone 6 Tenmoku. Each of these pieces is a thin slab of white porcelain, less than 1/4" thick which had a very angular look. But after firing you can see all the pieces have puffed-up like a pastry and rounded out, with the base warped into a curve.

I'm starting a piece with what I think is Laguna WC-437 Frost Porcelain, but it's labelled Cone 5, so I will be interested to see how it fires.

I've also experienced bubbling problems with porous cone 10 clay with a cone 6 glaze fired at cone 6. The clay never densifies, so the glaze infiltrates so deeply into the bisque, vertically as much as 3 inches within the bisque, that the glaze reaction off-gases all through the piece with pinholes everywhere.

Hey Norm, Thanks for the reply. I have tried refiring pieces with slight glaze anomalies and they come out with bubbles surfaces.  I continue to be amazed at the myriad ways of clay . . .

I am about to fire another load of the cone 4-6 porcelain at a slightly lower temp - I live in fear and trepidation!

We have a 2005 copy of "Ceramic Faults and Their Remedies" at our studio. It's helpful.

After showing this book to a artist raised on Harry Potter he said, "Wow! This is like a book of Curses and Counter-Spells."

http://www.amazon.com/gp/product/0713671912/

Looks like a good resource. I just ordered a copy.

Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service