I've having major pin holing issues with  the Sapphire blue (revised) glaze recipe from Ron Roy's web site Frog Pond Pottery. It's happening both with a standard slow pre-programmed Bartlett firing & with a custom controlled cool/slow glaze firing. Should I be holding it longer @1900 &/or 1400 to let all the gasses release? It's only happening with the Sapphire glaze. Or should I create  a new custom firing schedule?
I  even bisqued my last greenware at ^04 and it still didn't help. It's happening on both hand built & thrown pieces mostly on the red body clays. Is it just a case of a bad fit of the glaze & Clay body?
Any help or suggestion would be greatly appreciated as it is a glaze that I love dearly!!!!

Views: 1064

▶ Reply to This

Replies to This Discussion

Juanita:

you said " major pinhole" problem. Does that means numerous pinholes or large pinholes= blisters? A picture would certainly be helpful. Pin holes are most commonly from off gassing spars: mostly Nep Sy in the clay. However, you are using a red clay body: which means it could be a sulfide problem. Red and dark body clays equal higher iron, which in turn means high sulfide content. The solution for off gassing pinholes and the solution for sulfide blistering is not the same.

you can start here and check results. Use your current slow firing schedule, but ramp at 125F an hour from 2050 to 2230F. At 2050F the clay body starts to vitrify, and the porosity begins to close as glass forms. At 2000-2050F is also when spars reach their most active state: which also means increased off gassing. So going slow from 2050F to peak allows the body to mature, as it also allows the time for spars to off gas.

Now once you fire this schedule and you still have noticeable pinholes: then sulfides become the prime suspect. Sulfides mimic off gassing spars: but require a different schedule to resolve. Red and dark bodied clays are the most likely suspects to have sulfide issues. 

Tom

i have a blog floating around here someplace called " clay tips for potters." There is a lengthy post on firing red/ dark bodied stoneware. 

By the way: next time I talk to Ron I will tell him to fix his recipe. :)

Numerous tiny pinholes!!!! I really think it is coming from too thick of an application cause there's little to none where it is thin. Unfortunately, it's not blue enough when applied thinly.

I don't think there's an issue with the glaze recipe itself.

I shall look at my firing schedule and maybe re program. I fire a lot of semi-matte  & glossy glazes in the same load and don't  want to mess with the results I've been getting so far. 

I'll take a few photos & post if I can focus in on the pinholes without glare from the glossy surface 

I think the recipe is fine as it is

I was joking about Ron :)

Just had a quick look at the blog. Looks very complex. I'll give it a thorough read when I can concentrate. Hot & muggy in my neck of the woods right now!!!!

George Lewter said:

Attachments:

The glare from the glossy surface made it difficult to photograph the pinholes. They're tiny & all over

▶ Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service