hello all,

has anyone experimented with jan's dryglaze recipe - wondering if anyone knows the equivalent for frit 4193 - we are looking for a USA frit that is equivalent for her frit 4193.  thanks, carol

Views: 912

Reply to This

Replies to This Discussion

Since the recipe uses just 8% Ferro Frit 4193, you can substitute Ferro Frit 3124 which will function similarly.

3124 melts at a nearly identical range, having 44% more refractory alumina which is offset by containing 50% more calcium oxide flux with 3% less Boron.

http://janwallacepottery.blogspot.com/2012/04/mucking-around-with-d...

As with substituting for the MOK-632 frit Alisa Claussen uses, you may want to make certain additions as both 4193 and MOK-632 contain Zinc Oxide and Barium Oxide, not typically found in American frits. For most glazes leaving these out doesn't make a difference, but in some glazes you need to add either the zinc or barium or both to replicate the look.

At the 8% level used in her recipe, this would be 0.22% zinc oxide and 0.16% barium oxide. Very small quantities. The extra calcium in the 3124 will more than provide the same additional semi-matte look zinc would supply, but zinc and barium both create color changes in many colorant oxides.

http://digitalfire.com/4sight/material/ferro_frit_4193_2980.html

http://digitalfire.com/4sight/material/ferro_frit_3124_350.html

Just the sake of information, this is the substitution I use for MOK-632.

It over-supplies Calcium Oxide which in some glazes can be removed by reducing other ingredients.

MOK-632 Substitute

75.0%    Ferro Frit 3134
30.0%    Borax
10.0%    Soda Ash
5.8%      Zinc Oxide
5.3%      Strontium Carbonate or Barium Carbonate
-12.8%  Calcium Oxide

Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service