I am using 3134 instead of 3124 in the SCM formula. Does anyone know if this will result in anything unfavorable?
Thanks - Paul

Views: 5131

Reply to This

Replies to This Discussion

Ferro Frit 3124 has alumina and melts at ^05, while 3134 has no alumina but more borax and calcium flux so melts at a much lower temperature of ^015.

3134 with kaolin is a perfect glaze base, so we use it in far greater quantity than other frits. If you ever want an even more fluid glaze, turn to frits with fluorine like 3269 or 5301.

Due to the alumina and less flux 3124 tends to make stiffer glazes while melted. Mastering Cone 6 Glazes use 3124 for their ^6 Majolica, which is a very stiff, hard glaze which tends to crawl.

Thanks Norm for the info! So if I understand correctly, 3134 in substitution for 3124 in SCM, I may see a less matte surface, which for me is not a problem. I think I'll proceed and see what happens. Thanks again!
Paul

It will be interesting to see what happens. Taking a chance on a small batch of something new is the only way to discover something no one has seen before.

SCM (Strontium Crystal Magic - cool and warm) is a fluid underglaze which interacts with the glaze on top, giving it more flow and crystallization. Sometimes I wish it imparted less flow, and this change may do that.

A similar situation are the two layer oil spot glazes. I found the top layer looks great on any red iron oxide glaze (red iron oxide is refractory at ^6).  I made the original base layer with black iron oxide (a flux at ^6)  and it provided so much flow that the top layer of oil spot glaze slid off the ware during the firing except where it was perfectly flat.

Reply to Discussion

RSS

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2026   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service